![]() Home |
| ![]() Home |
The KAISER - EFFECT and its Scientific BackgroundHans Maria Tensi PrefaceThis paper is given on the occasion of honouring Joseph Kaiser with a festival event at the '26th European Conference on Acoustic Emission Testing' in Berlin, Sept. 2004 and the granting of a commemorative plaque to the Technical University Munich (TUM), the birthplace of the AE-technology, by the 'Acoustic Emission Working Group', USA. Outline of this PaperWith this presentation three goals shall be achieved: - Firstly important facts from the works of Joseph Kaiser will be presented, which lead to the discovery of the "KAISER-EFFECT". I also want to emphasise the severe technical and organisational problems in Germany during 1945 - 1950. - Secondly I want to define exactly the phenomenon of the "KAISER-EFFECT". This effect has already been studied in the sixties and seventies of the last century and I shall refer to experimental results from that time. - Thirdly I will describe the solid-state background of the acoustic sound emission (ASE) during mechanical load of metals and alloys. Additionally this analysis is correlated with other sources of an ASE. Results of newer research are mostly presented schematically. This paper is not intended to be a summary and aggregation of the literature from this area. The few references are fundamental research papers directly covering this topic. 1 Work of Joseph KaiserDirectly after world war II in 1945 Dipl.-Ing.(Univ.) Joseph Kaiser visited the chair of the mechanics, Prof. Dr.phil. Ludwig Föppl. He asked him, whether he could do research on the sounds which metals issue upon mechanical stress. The so-called "tin-clamour" had already been known in the middle ages. Tin-casters had manually cambered used tin plates and listened to the "clamour". Thus they could estimate the material quality of those plates given to them for melting. The sound revealed whether the plate contained many impurities, for example, like Pb and Zn - disallowed even then - which would reduce the brilliance of the new castings. In 1945 two points made the project very questionable: could the technical effort for the measurements be done in post-war Germany and are there at all other technical interesting metals who would issue sounds? One has to imagine the situation at that time: Munich and the Technical University in its centre were destroyed to about 80%. Figure 1 gives an impression of the TUM in 1945. Of course the circumstances for such an innovative research were pretty bad! 31 DGZfP-Proceedings BB 90-CD Keynote EWGAE 2004 Figure 1: Technical University of Munich (TUM) destroyed after the World War II in the time of 1945/46: The 'Auditorium Maximum', behind institutes and laboratories; in front of all one of the famous two 'Rosselenker' (leader of a horse). Quelle: Münchener Stadtmuseum, Archiv für Fotographien Figure 2: Cover page of Kaiser's doctoral thesis from February 15th 1950; library of the Technische Hochschule München 'Diss.10/1320' 32 DGZfP-Proceedings BB 90-CD Keynote EWGAE 2004 Figure 3: Photography of the first experimental set-up to measure the Acoustic Sound Emission (ASE) with pendulum tensile machine, amplifier and oscilloscope from 1949; J. Kaiser 'Diss.10/1320' Figure 4: Experimental set-up of tensile probe's clamping with the piezo-microphone in the tensile machine; J. Kaiser 'Diss.10/1320' Nevertheless Föppl had a fundamental scientific interest in researching the backgrounds of technical materials' behaviour under mechanical stress. Such research had been done world-wide at that time. Only little was known on the processes in the crystal lattice upon deformation. Hence Prof. Föppl gave his approval and Kaiser could start with his work. First we ought to pay attention to Kaiser's doctoral thesis, which was finished in early 1950. Figure 2 shows the cover of this work. At first Kaiser had to build his devices from fragments of obsolete military equipment. He built piezo-crystal microphones from quartz- and seignette-crystals, all electronic devices (e.g. a DC- amplifier with a maximum amplification of 106) and as displays for the acoustic signals an oscilloscope with an old Braun tube. About in 1947 his first experimental setup was completed (Figure 3). This setup was continually improved (especially when better-suited parts had been available). The figure shows an old pendulum tensile testing device, which could only be manually operated because of the background noise. The specimen had the tightly fitted microphone at its top (figure 4), the signals were transferred via a pre-amplifier (VV) and a main-amplifier (HV) to the oscilloscope. There was a hard and nearly unsolvable problem remaining: how to record and sample the signals permanently? The institute had a cine camera with a continuous film transport (with max. 30m/s). When switching off the time sweep in the oscilloscope, this could serve as a signal sampling and registration device in principle. 33 DGZfP-Proceedings BB 90-CD Keynote EWGAE 2004 Figure 5: Stress-strain diagram of a tensile probe for soft carbon steel with triple photographs of the screen of the oscilloscope (with time sweep), assigned to points of the stress-strain function; J. Kaiser 'Diss.10/1320' 34 Unfortunately the camera could only record for about 30 seconds which was too little in comparison to the length of a tensile test. Also because of the infernal noise produced by the camera, such registration was out of the question. At least Kaiser could use this signal registration method for checking his self-designed piezo- microphones. To give an impression of the effort and hardship of analysing the registered high-frequency signals, at that time all photographs from signals shown in the Braun tube had to be analysed by a measuring stick! Finally a 16mm-cine camera acted as a sufficient makeshift to record the ASE of complete tensile tests. Its mechanical transport mechanism did not produce loud noises. The oscilloscopes time sweep was activated during the experiments. Figure 5 shows the example of a successful experiment. Kaiser told that typically many experiments had to be done until all components of the setup were simultaneously (!) working correctly: When testing the specimen from soft carbon steel, the load- elongation-function shows the linear Hook area and at its end a distinctive yield strength. After that there is a monotonous increase in load with discontinuities of the 'Portevin-le-Chatelier- effect' (also 'strain-induced aging'). For some selected points of this function we show how each is represented in three pictures of the camera, recording the display of the Braun tube. This means the sampling is done within a time period of 3 x 1/25s approximating a point in time. Those pictures were analysed for 'jumps', 'amplitude' and 'frequency' of the signals with a measuring stick. The result of this tedious analysis is shown in figure 6 (all evaluated characteristics were plotted against the load or the fictitious stress): The amplitude function shows an oscillation with three maxima, the frequency (in Hz) only has a maximum at about 7500kN. The position of the highest frequency matches the position of the distinctive yield strength. DGZfP-Proceedings BB 90-CD Keynote EWGAE 2004 Unfortunately due to the significant size reduction of the original picture, this cannot be satisfactorily recognised here. Another problem were the low resonance frequencies of the microphones, which were even decreased by the mechanical fitting to the specimen! Hence eight years later a qualification of the ASE was done by a comparative energy measurement (where the acoustic energy is assumed to be proportional to frequency x ampli- tude). In his dissertation Kaiser examined different metals and alloys and even organic materials, like wood. The most important consequence of Kaiser's dissertation can be found on page 27, line 7 to 10. Here he describes the effect when a specimen having been loaded to 500kN before was loaded again over this previous maximum load. The original words from Kaiser: Figure 6: Analysis of Figure 5; J. Kaiser 'Diss.10/1320' Figure 7: The effect to determine the previous load on a probe by measuring the ASE, first described in Dr. Joseph Kaiser's doctoral thesis 1950; J. Kaiser's Patent 'Nr. 852 771 - Kl.42 k Gr.3401' 35 DGZfP-Proceedings BB 90-CD Keynote EWGAE 2004 »Bei einer nun folgenden Wiederbelastung traten nur vereinzelt Sprünge auf, bis die ursprüngliche Belastung von 50kg wieder erreicht war und sofort war die Wirkung der Effekte in ihrer ursprünglichen Heftigkeit wieder zu erkennen.«1 And in the summary of his dissertation on page 37, second paragraph, line 1 to 4: »Ein wichtiges Ergebnis der angewandten Versuchsmethode ist die Tatsache, daß nachträglich, ohne den Prüfling zu zerstören, sich Aussagen machen lassen über die Höhe der höchsten Belastung, die das Material bereits ausgehalten hat. Also die Kenntnis der Beanspruchung, die auf dem Material war und nicht nur augenblicklich ist.«2 Those statements were the basis of the great success of his ASE-measurements in the area of non-destructive material tests and are the core of the 'KAISER-EFFECT'. For that reason Dr. Joseph Kaiser got a patent on his method for registering the ASE upon mechanical loading of materials, Patent Nr. 852 771 -Kl.42 k Gr.34 01". Figure 7 (taken from this patent) describes, how the absence of ASE was exemplified by a tensile test, done by Kaiser. During the very few days of the formal hand-over (in 1957), caused by his severe illness, Dr. Kaiser told me about a spectacular success of his method: In the United States a big pressure tank had burst although the manometer had shown that the specified maximum load had not by far been reached. Kaiser took tensile speci- mens from different areas of the burst wall of the pressure tank. Apparently he took enough specimens and also at the relevant positions to do a stringent analysis. By his ASE-analyses of these specimens he could prove that indeed the tank wall had not been overstrained at any time. But the specimens from the support area were definitely overstrained! The tank had unnecessarily been welded to the support construction which could later be verified. The strain peaks - originating from welding - were the cause of the catastrophe! Dr. Joseph Kaiser passed away in March 1958.
1 »By a new reloading [of the tensile specimen] only few jumps occurred [in the photograph of the Braun valve] until the loading reached the former highest level of 50kg and immediately the impact of the effects [acoustic sound emission ASE] could be observed with the former vehemence.« 2 »One important result of this developed testing method is the fact that the ex-post statements can be made about the maximum of load, which the material has endured before, without destroying the probe. Also the knowledge of the stress, that had laid on the material and not the stress, which exists at the moment.« Figure 8: Dr. Joseph Kaiser giving a lecture at the Technical University of Munich (TUM), Institut für Metallurgie und Metallkunde, about Acoustic Sound Emission during tensile testing; about 1955; private photos of the institute (R. Meier) 36 DGZfP-Proceedings BB 90-CD Keynote EWGAE 2004 2 ASE experiments with mechanical loading of metals and introduction of the term 'KAISER EFFECT'When in 1957 I was offered to do further research on those - at that time - unusual effects I did some changes in the equipment: First of all the old pendulum tensile test machine was replaced by a hydraulic machine with a big oil accumulator tank. Via a special designed valve system, the oil pressure could be applied to a floating working piston, such that its stroke remained constant for different velocities and for loads up to 10kN along the elongations to be expected. Of course during the experiments the pumps were switched off. Since there were many specimens made of different alloys and different kinds of heat treatment the clamping was changed to also allow flat specimens. At first I abandoned Kaiser's claim of gathering a lot of experimental parameters (like graphical sampling of jumps, frequency and amplitude) and simply measured the ASE with an electronic counter for frequency and amplitude. All tensile tests revealed similar diagrams as can be seen in figure 9 for a soft-annealed steel specimen with 0.15%C, which had been grinded extremely scale-free. In close conformance to Kaiser, the ASE maximum is in the elongation area of the distinctive yield strength. The little ASE in the Hook area is rather to be explained by faults in the experimental process (like imprecise clamping, the floating working piston or some deformed specimen). After passing the distinctive yield strength, the ASE falls exponentially in the area of strain-hardening and a potential 'Portevin-le-Chatelier-effect', with following reduction of the cross sectional area. Finally there is an extreme peak in the ASE at the fracture point which comes mostly from the machine. Figure 10 shows schematically the ASE and the stress as functions elongation stress ASE intensity Figure 9: Stress-strain diagram and ASE-strain diagram of a soft-annealed steel probe with 0,15 wght% carbon; H. M. Tensi's doctoral thesis 1960 previously applied maximum elongation elongation after first load application elongation stress Figure 10: The KAISER EFFECT, schematic from Figure 9; H. M. Tensi's doctoral thesis 1960 Z ASE intensity 37 DGZfP-Proceedings BB 90-CD Keynote EWGAE 2004 against the elongation for a tensile test specimen, which has already been loaded up to point "Z". Clearly the sudden ASE increasing upon passing the previous load can be recognised. With those kinds of diagrams (also of specimens with multiple step-like loads) since about 1961 I established the so-called KAISER-EFFECT and propagated it in publications and lectures on international conferences to honour Kaiser's pioneering work, with the support of my doctoral advisor, Prof. Dr. Heinz Borchers. stress ASE intensity ASE intensity stress elongation area of KAISER EFFECT a) area of KAISER EFFECT b) Figure 11a and b: Areas in the scales of stress and of elongation for using the KAISER EFFECT For illustration, figure 11a and b show the areas to use the KAISER-EFFECT as shaded for functions plotted against loading or elongation. 3 Reasons for ASE during mechanical loading of metals3.1 Dislocation reactions and 'up-hill-diffusion'To understand the background of ASE different metals and alloys with different kinds of heat treatment were analysed with tensile tests. The at that time confirmed knowledge had been that the ASE intensity has its maximum for an occurrence of a distinctive yield strength, i.e., during the extremely inhomogeneous plastic deformation. Hence different materials with different heat treatment and significant differences in the yield strength formation were compared with respect to their ASE (figures 12a to d). As one can clearly recognise, the maximum of the ASE in width and height decreases with the decrease of the yield strength elongation: from carbon steel (figure 12a) over differently heat treated aluminium alloys (figures 12b and c) to pure aluminium (figure 12d). Pure aluminium has - after being high-temperature-annealed with abrupt quenching - not only the least strength but high ductility, but also the least ASE. Those and other metallurgic research revealed that the ASE is strongly influenced by inhomogeneous slip of the so-called slip dislocation. Dislocations are considered to be the only medium for plastic deformation in metallic crystals. 38 DGZfP-Proceedings BB 90-CD Keynote EWGAE 2004 a) carbon steel stress ASE elongation b) aluminum alloy - aged stress ASE stress ASE stress ASE c) aluminum alloy - soft annealed d) pure aluminum - annealed and quenched Figure 12a - d: Differences in yield strength elongation and ASE of different materials and heat treatments to show the connection of yield strength and ASE; H. M.Tensi's doctoral thesis 1960 a) b) Figure 13a and b: Reaction of dislocation on a slip plane of a metal with impurity atoms a) the impurity atoms are distributed homogeneously; the dislocations are not blocked b) the impurity atoms create clusters at the dislocations and block them; by increasing stress the dislocation suddenly jumps out of the Cottrell cloud 39 This can be illustrated with a simplified model (see figures 13a and b): When applying a force the dislocations slip on so-called slip planes within the crystal. They distort the crystal- lattice in their environment with fields of pressure above, fields of tension below the slip-plane. In figure 13a the dislocations slip exactly for one lattice distance 'b' when a load is applied. Homogeneously distributed impurities will not disturb their movement. Integrating those multiple dislocation reactions, the material will deform very steadily. Now consider a heat treatment which allows a so-called 'up hill diffusion' of the impurities. They will diffuse to the lower side of the dislocation, where there is a local field of stress (figure 13b). The impurities are now distributed inhomogeneously near the dislocation. This causes a release of tension and the dislocations are blocked in their mobility. The local amount of shear stress increases, until the blocked dislocation is torn off of its so-called "Cottrell cloud" and it jumps over several lattice distances (n x 'b'). This causes minuscule concussions in the metal which combine to the ASE. Those models were later confirmed by specific solid-state analyses (e.g. with an electron microscope). DGZfP-Proceedings BB 90-CD Keynote EWGAE 2004 To reinforce that theory about the ASE, tensile tests were done with the same material but with differently distinctive yield strength elongation. Those differences in the elongation for the yield strength were produced by heat treatment with materials with interstitial but also with substitutional impurity atoms. Flat tensile test specimens from a technical AlMg3-alloy were at first heat-treated uniformly such that all impurity atoms (also the Mg-atoms) were homogeneously distributed within the crystal. Then several groups of specimens were differently heat-treated to produce different levels of "up-hill-diffusion". As had been expected from the theory (see figure 14), with little deviation the ASE in specimens with zero elongation of the yield strength and no "up-hill-diffusion" (i.e. an ideal distribution of impurity atoms) increased monotonously to the specimens with the highest level of "up-hill- diffusion" (and blocked dislocation). 3.2 Stress ASE caused by other events in materials and constructionsIn practice there are very seldom those simple materials we had during research where the theory can be applied without modification. When you want to apply the ASE measurement, it is important to know the history of the material: its production as well as all its treatment when constructing the final technical product. Also one has to consider all imaginable stress conditions of the part in operation e.g. corrosion with or without mechanical load. Besides the dislocation reactions described above, figures 15a and b sketch some also important microstructure properties, which affect the triggering of the ASE. At position 1 there is a so-called micro-cavity (note that there are no macro-cavities, since we assume that the material is fault-free in a technical sense). The micro-cavity is caused by the solidification and normally cannot be prevented. Even when the casting material is post- processed by heat and/or mechanical treatment, removal of the micro-cavities is impossible without leaving other faults. Such cavities are characterised by extremely sharp notches. Already for a very small mechanical load the local stress accumulates near this notch because of the so-called 'notch-stress' (after H. Neuber). Dislocation processes (as described above) start very early in those areas, even when the part is still for most of its volume in its elastic deformation phase (where the Hook law applies). Additionally those notches tear open and the surface of cavity gets larger (figure 15b). When the load of the part (or specimen) vanishes, those exposed surface fold up. When a reload is applied those planes are separated again. This causes rubbing noises with additional ASE, even though the previous load has not yet been exceeded. ASE 5 x106 4 (number of signals) 3 2 1 0 20 40 60 80 100 yield strength elongation in percent of highest value Figure 14: ASE in dependence of the length of the yield strength elongation (or the increasing 'up-hill diffusion') showing the influence on the ASE by blocked dislocations. H. M.Tensi's doctoral thesis 1960 0 40 DGZfP-Proceedings BB 90-CD Keynote EWGAE 2004 load load 1 3 2 3 4 Figure 15a and b: Metallurgical irregularities in the structure of technical materials contributing to the ASE 1: micro-cavities; 2: internal cracks and fissures; 3: inclusions e.g. metallic and non-metallic phases; 4: external cracks a) without external load; b) with load applied This example makes clear what kind of sources the ASE has: normal dislocation reactions, reinforced dislocation reactions caused by the 'notch-stress' and repeated tearing open of notches followed by folding up of the cavity flanks: the KAISER-EFFECT blurs for reloading. At position 2 in figure 15a and b there is an internal crack: It can be so minuscule that it is invisible even for ultrasonic. But it will cause the same effects causing ASE as the cavity. At position 3 in figure 15a and b there is an inter-metallic phase having a needle or plate shape from its formation or from hot rolling. Inter-metallic phases (IP) typically have no ductility, this causes their extreme brittleness. They are mechanically comparable to a crack in the grid (see above). Additionally they have a very weak connection to the interface of the lattice such that they behave like a crack. All mechanisms of ASE triggering described above can be applied here. The refractory IPs may break and cause cracks or additional sharp edges which multiply those effects. At position 4 there is an external crack. This may be caused by leaking dislocations (so called extrusions) often in combination with corrosion. This is the dangerous 'stress-corrosion', where crack graving is exponential. The tensile test for such a specimen also shows only a blurred step in the ASE-function and thus only an indistinct KAISER-EFFECT. A simplistic interpretation of the KAISER-EFFECT is not appropriate here, because when you ignore the stress-corrosion before you would expect a distinctive KAISER-EFFECT. Hence whenever you find this behaviour of ASE it may be an indication of stress-corrosion! The theory presented above has been proven correct in many situations from practice. 4 SummaryIn this paper the cornerstones of the work of Dr. Joseph Kaiser were described as far as necessary to understand the KAISER-EFFECT. I have mostly reverted to original presentations of Kaiser. This should also emphasise the nearly unimaginably hard circumstances of his research in post-war Germany. 2 4 a) without any external tensile load 1 b) 41 DGZfP-Proceedings BB 90-CD Keynote EWGAE 2004 Newer measurements have revealed dislocation reactions as the cause of the ASE and proposed the term 'KAISER-EFFECT' to honour his pioneering work. Additionally fundamental and other sources of ASE have been described which can be found in real technical materials. Literature1) J. Kaiser: 'Untersuchung über das Auftreten von Geräuschen beim Zugversuch', Dr.-Ing. Dissertation, Fakultät für Maschinenwesen und Elektrotechnik der Technischen Universität München (TUM); 15.2.1950 — 2) J. Kaiser: Patentschrift der Deutschen Patentamtes Nr. 852771, Klasse 42 k, Gruppe 3401 vom 20.10.1952 - 'Materialprüfverfahren' — 3) J. Kaiser: Arch. Eisenhüttenwesen 24 (1953) 43 - J. Kaiser: Forsch. Ing. Wesen (1957) 38 — 4) J. Kaiser: Bsp. angewandter Forschung 1957, Fraunhofer-Gesellschaft — 5) H. Borchers u. J. Kaiser: Z. Metallknde. 49 (1958) 2 — 6) H. M. Tensi: Piezoelektrische Impulsmessung zur Untersuchung von Vorgängen in Metallen bei Phasenänderungen und bei mechanischer Beanspruchung, Dr.-Ing. Dissertation, Fakultät für Maschinenwesen und Elektrotechnik der Technischen Universität München (TUM); 5.1961 — 7) H. Borchers u. H. M. Tensi: Z. Metallknde. 51 (1960) 212 — 8) A. H. Cottrell: Dislocations and Plastic Flow in Crystals, Oxford at the Clarendon Press, Amen House, London E.C.4, 1958, 223 pages — 9) C. Kittel: Einführung in die Festkörperphysik, R. Oldenbourg Verlag München u. Wien, 1969, 744 Seiten — 10) T. F. Drouillard: Acoustic Emission, a Bibliography with Abstracts, IFI/Plenum New York-Washington- London, 1979, ISBN 0-306-65179-3, 787 pages. 42 |
| © NDT.net |