The use of guided waves for non-destructive testing has become increasingly common over the past few years, as demonstrated by the UT Articles presented in the March issue of the UT Online Journal (ref.1), and by the Lamb Wave Bibliography (ref.2) of the same Journal. One of the aspects that make guided waves attractive for testing is their ability to propogate along surfaces over distances of tens of centimeters and therefore to allow a significant increase in scanning speed. Other aspects are the possibility of material characterization and economical flaw detection in layered media as used in the aerospace and petrochemical industries.
A prerequisite for the successful application of guided waves in most cases is a surface which does not damp the surface wave. This precludes the use of liquid couplants, therefore special dry coupled transducers must be used. Alternatives can be found in laser generated (ref.3) and air coupled ultrasound. Air coupled ultrasound with transducers having stand-off distances in the centimeter range, and which are already used by the industry in the through-transmission configuration (ref. 4), are well suited for guided wave applications.
|
The impedance mismatch between air and transmitter/receiver and, more importantly, between air and test part introduces total reflection losses in through transmission which can exceed 120 dB (for more details see ref.5).
Although matching layers on the transducers can reduce these losses by about 40 dB, more sophisticated measures must be taken in order to receive a signal with an acceptable signal to noise ratio. On the transmitting side, high sound pressures are generated by a resonant transducer with a focused beam profile (figure 1). The transducer is driven with tonebursts of 400 kHz with 15 cycles at a repetition rate of 300 Hz (figure2). The same transducer design is used on the receiving side. The received signal is pre-amplified (yielding a signal to noise ratio exceeding 40 dB), then further amplified by a super-low noise amplifier. Both transducers are 25 mm in diameter and spherically contoured with a focal length of 38 mm, resulting in a focal spot in air of 1.3 mm. The control unit (SONDA 007C) provides for fine tuning of the transmitter driver and the receiver bandpass to the respective resonant frequencies. 3. TRANSDUCER CONFIGURATIONS AND WAVE MODESAir coupled transducers can be aligned in several ways, as shown in figures 3 and 4. Figure 3: Bulk Waves. a) Through-transmission compressional wave. b) Through-transmission shear wave. c) Pseudo pulse-echo with a sound barrier between transmitter and receiver. Figure 4: Guided Plate Waves. a) Transducers on same side (one-sided). b) Transducers on opposite sides (two-sided).
The various configurations are named according to the wave modes that are generated, analogous to contact transducers. Conclusive evidence for certain modes exists in some cases, while investigations are in progress for more complex test structures. In all the cases here presented, flaws could be detected reliably - even if the active wave modes were not known with certainty.
![]() ![]() ![]() ![]()
|
Several nondestructive methods were subsequently evaluated in order to detect these microcracks. Among the methods that failed to detect those flaws were X- ray holography, micro focus X-ray, ultrasonic water squirters, shearography, mechanical impedance, and acoustic impedance.
Detection was possible with the air coupled technique. The guided plate wave configuration was used with the transducers on opposite sides (Fig. 4b). The transducers were adjusted to form an angle of 10 degrees to the normal, and the distance between the focal points on the part was 10 mm.
Fig. 5a shows the C-scan image of an intact Gr/Ep laminate before thermocycling (dimensions: 150 mm x 150 mm, 0.15 mm thick; step size 0.5 mm, scan speed 76 mm/sec).
Fig. 5b shows the same sample after thermocycling. Note the fine horizontal blue lines. Material analysis and visual inspection with magnifying glasses identified these lines as microcracks.
Fig. 6a
Fig. 6b
Fig. 7
Considering the thickness d of the composite face sheet (0.15 mm) and the aluminum core (0.018 mm) raises questions about the transmission mechanism of the ultrasonic waves. The following table lists sound velocities (CL : longitudinal, CT: compressional wave) and wavelengths l for the air scan frequency of 0.4 MHz.
| MATERIAL | CL [m/s] | C T [m/s] | f [MHz] | [mm]
| d [mm] |
| Air | 340 | na | 0.4 | 0.85 | 38 |
| Composite | 3000 | 1500 | 0.4 | 7.5 | 0.15 |
| Aluminum | 6400 | 3040 | 0.4 | 16 | 0.018 |
The ultrasonic wavelengths of 7.5 mm and 16 mm are orders of magnitudes larger than the material thicknesses of 0.15 mm and 0.018 mm. Consequently, neither compressional nor shear waves can be involved. Plate or surface waves must be considered as possible transmission mechanisms. Figure 8a shows in a sketch how plate waves (symmetrical and asymmetrical) could be generated directly or by mode conversion. The face sheet is shown with asymmetrical plate waves, while the aluminum core is shown with both asymmetrical (left side) and symmetrical (right side) plate waves.
![]() |
|
Plate waves can be described by the following Rayleigh-Lamb equations (ref. 3):
tanh qh / tanh ph = 4k2pq / (q2 + k2)2 : symmetric modes
tanh qh / tanh ph = (q2 + k2) 2 / 4k2pq : asymmetric modes
p2 = k2 - (w2 / c2L ) |
k = 2 / : wavenumber = 2 f : angular frequencycP = / k : phase velocityh : half plate thickness cL : longitudinal velocity cT : shear velocity < |
The dispersion curves, displaying the relation between phase velocity of the various lamb waves a0, a1, a2, ... and s0, s1, s2, and the product of thickness d and frequency f are shown in figure 8 (ref 6). For the aluminum core mentioned in the above table, the product d*f equals 7.2 m/s, which coincides with the ordinate in figure 8. Only the symmetrical s0 or the asymmetrical a0 mode is therefore possible in the aluminum core. According to the above equations the phase velocities are:
Observations of time of flight indicate a velocity in the range of several thousand m/s. The asymmetrical plate wave is too slow, therefore the ultrasound is transmitted through the core by the symmetrical plate wave.
Strong evidence for the involvement of plate waves in the testing of honeycombs by air coupled techniques was obtained when testing the honeycomb sample, which was manufactured by using the face sheet with the previously observed microcracks (figure 5b).
Fig. 9
The honeycomb sample was scanned with the transducers in the through transmission configuration (fig.3a), and the C-scan image is reproduced in figure 9. Note the black horizontal lines. They coincide with the microcracks detected in the face sheet using plate waves. The fact that the same cracks appear now with the through transmission configuration is believed to be possible only because of the existence of plate waves.
More precise measurements and additional investigations are needed to fully understand the variety of modes and mode conversions that are very likely to occur in honeycomb structures.
| Willem A. Grandia, P.E. Bill Grandia is founder and president of QMI, where he directs R&D. He is a senior electronic and quality engineer, recognized worldwide for his achievements in designing ultrasonic and Eddy Current instrumentation. He started his career in 1955 in Holland. | Jan Strycek Jan serves as Vice-President for Technique Development and Marketing. He acquired in over 25 years an outstanding record in practical testing of a large variety of materials and structures. Jan is recognized and called upon worldwide as an expert for the most difficult and critical NDT tasks. Author moved to: jan@airstar1.com or http://www.airstar1.com | Hanspeter Loertscher Hanspeter joined the company 2 years ago. He received his Master Degree in Physics in 1972 from the University of Bern, Switzerland and is specialized in laser development and applications, including laser based ultrasonics, and in ultrasonic testing of composite structures. Author moved to: hanspeter@airstar1.com or http://www.airstar1.com |
The paper was presented on the Application Workshop in May '97 |Top to this page|