Re: UT Cal Blocks for Piping / Curved Surfaces

Posted by: Ed T. Profile (PID_1936), E-mail: ndtsolutions@yahoo.com, on November 25, 2004 at 13:22 :

In Reply to: Re: UT Cal Blocks for Piping / Curved Surfaces posted by : General , E-mail: iclampers@hotmail.com, on November 25, 2004 at 12:42 :

----------- Start Original Message -----------
: So then every diameter and every schedule needs its own cal block. I dont think they really thought that through well when they changed that. It used to be 6 cal blocks would cover you for all diameters for a specified thickness but now you need every one to be individual, wowzers.
: It does make sense since it is more of a true representation of your test piece but for the tech now it means carting around a whole bunch more blocks.
: Thanks for your reply, I appreciate it.
:
: : : First I want to thank everyone who have been replying to my posts lately. It has beeen a great help for my questions.
: : : I'm hoping someone can help me here as well.
: : : Well dealing with piping / curved surfaces 20" diameter and less ASME V requires you to use a curved cal block and they show a diagram for it and stipulate the diameter limitations it can be used for (0.9 - 1.5 times the diametr of the cal block). My question is, what about the thickness range for the curved cal block? Do the curved blocks follow the same requirements as the non curved blocks (ie; up to one inch use a 3/4" or t thickness cal block).
: : : I would really appreciate some input on this as I am very confused. Thanks.
: : Hey Ice. I am looking at ASME V, Article 4, 2002 Edition. The diameters for curved surfaces 20” and less are not applicable to piping. The block thicknesses and Block range of use described in T-434.2.2 & T434.2.3 are applicable to non piping applications only, such as vessels.
: : For piping you must refer to T-434.3. This states “The basic calibration block shall be a section of pipe of the same nominal size and schedule”.
: : Then it refers you to Fig. T-434.4.1.
: : Ideally the calibration block would be a sample of the material to be inspected, as required by API-1104 for pipelines. However, that would not be practical in a power plant.
: : But to answer your question, you are correct. You would need a separate calibration block for each of the pipe sizes and schedules you described. The 4” NPS schedule 40 is not acceptable for use to examine the 4” NPS schedule 80 or 160.
: : You would need 2 additional calibration blocks.
------------ End Original Message ------------

Yoou're welcome. But remember, that is for piping. If you are examining non-piping the 0.9 to 1.5 applies.



Follow Ups:



Post a Followup:

Name:
E-Mail:

Subject:

Comments:

Optional Link URL: Example: "http://www....html". Alternative write "http://www.ndt.net/wshop/attach/filename.htm" if you transfered a filename.htm via FTP
Link Title: is important! Information on my Home Page
Optional Image URL: http://www....gif


Attention! Please click the button only once. This may take a moment to process


[ Technical Discussions ] [ All Message Boards ] [ Help ]