10:39 Mar-19-2009
SCC crack detection in SS

We have witnessed SCC in one of our columns, the cause of SCC is the Chroride presence in wet insulation. Now what NDT is usefull to detect the extent of attack quickly & effectively. PT we have done, MT is not applicable, How about Phased Array Eddy Current, is it sensitive enough to detect micro cracks, what about Omniscan. Do you think Metallography would help.

 
 Reply 
 
J. Mark Davis
Teacher, And Consultant
University of Ultrasonics, Birmingham, Alabama, USA, Joined Mar 2000, 85

J. Mark Davis

Teacher, And Consultant
University of Ultrasonics, Birmingham, Alabama,
USA,
Joined Mar 2000
85
12:22 Mar-19-2009
Re: SCC crack detection in SS
In Reply to faran at 10:39 Mar-19-2009 (Opening).

Detection of SCC for your application can be accomplished with OD Creeping Waves very effectively. OD Creeping Waves have been demonstrated to detect cracks on the scanning surface with a depth of 0.005 inches and less.

Phased Arrays are equally effective for detection and sizing of SCC. Even Phased Array using Creeping Waves would be effective.

Some questions are: what is the material type and what is the thickness.

Is detection your only concern. Do you need to size these Stress Corrosion Cracks.

What is your Critical Flaw Size?

To conclude this is a very easy application using Conventional OD Creeping Waves or using an OmniScan Phased Array System. The images you will get with the OmniScan will significantly help with detection and characterization.

Sincerely,

J. Mark Davis

 
 Reply 
 
Luis Ganhao
Engineering,
USA, Joined Sep 2008, 25

Luis Ganhao

Engineering,
USA,
Joined Sep 2008
25
15:02 Mar-19-2009
Re: SCC crack detection in SS
In Reply to faran at 10:39 Mar-19-2009 (Opening).

You can use TOFD to detect, size and carcaterized the SCC probably your unique limitation could be the thickness, however I could detect this kind of cracks in low thickness (9mm Lab testings). The setttieng-up (probes, frequency,size) is the clue for this application

 
 Reply 
 

Product Spotlight

Echomac® PA Tube Weld Tester

The new robotic Echomac® PA TW is an operator friendly test system for detecting weld zone defects
...
in tube and pipe caused by scarfing or welding processes. Electronic scanning ensures that the entire weld zone is covered without the need for mechanical movement or operator adjustment.
>

MANTIS

MANTIS is a compact, powerful and affordable flaw detector (16:64PR), dedicated to field operators
...
. This portable equipment offers standard (electronic-, sector-, compound scan, conventional UT for pulse-echo, dual array and TOFD inspections), and advanced phased-array (real-time TFM -Total Focusing Method). MANTIS benefits from the same intuitive and user-friendly interface (CAPTURE) than Gekko for easier inspections.
>

TraiNDE UT

TraiNDE UT is a virtual tool associated with a signal database which simulates real inspection con
...
ditions for numerous applications (Type A/V1 block, DAC block, welds and plates).
>

Conformable wedge transducer

The conformability is obtained with a flexible membrane filled with water between the transducer and
...
the inspected component. The coupling between the membrane and the component requires a small quantity of water or couplant. The conformable wedge combines the acoustic performance of immersion technique with good coupling and low attenuation.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window