Radiographic Examination of Weld in Pipes

WELDING OF PIPES
The bevels for GTAW Root pass as per ASME B16.25 is Fig No-5 and Fig No-6 for thickness of pipes greater than 10 mm. The figures indicate a cylindrical surface of 5 mm in the inside and also a broken line indicating the transition from the welding groove to the body of the component. We have adopted a transition straight away in the inside instead of 5 mm straight machining. We have now come to know that the straight machining of 5 mm is preferable when compared to that of tapered transition for radiographic evaluation. But we have been adopting this transition in many jobs without experiencing any problem in evaluation of the welding. We request your views on this . In case you feel the transition is OK without straight machining, please provide your view points for justifying the same since our customer feels that straight machining of 5 mm is preferable.


 
 Reply 
 
Doug Breeze
Director, Consultant; R&D
Inspection Software Limited, United Kingdom, Joined May 2000, 20

Doug Breeze

Director, Consultant; R&D
Inspection Software Limited,
United Kingdom,
Joined May 2000
20
06:00 Jun-06-2003
Re: Radiographic Examination of Weld in Pipes

The surface you describe is (or used to be!) called a counterbore. It has lots of benefits and few drawbacks, except for the machining costs...

1. Machining an identical counterbore on both joining pipes should prevent root-misalignment. This is leads to a more easily welded root-run, with less likelhood of root defects.

2. The counterbore provides uniform geometry on each side of the root so that radiography (and ultrasonic) inspection can more readily differentiate real defects from false geometric indications.

3. The counterbore reduces the included-angle at each root edge, and also distributes stresses adjacent to the root over a larger area thus minimising the risk of cracking and/or stress corrosion in this critical area.

Hope this helps.



 
 Reply 
 

Product Spotlight

Cygnus 6+ PRO Multi-Mode Ultrasonic Thickness Gauge

The Cygnus 6+ PRO thickness gauge is the most advance gauge within the Cygnus range with key featu
...
res including: comprehensive data logging; A-scan and B-scan display; manual gain control; Bluetooth connectivity; and much more. With its unique dual display and three measuring modes (Multiple-Echo, Echo-Echo and Single-Echo), this surface thickness gauge offers maximum versatility for inspections.
>

Conformable wedge transducer

The conformability is obtained with a flexible membrane filled with water between the transducer and
...
the inspected component. The coupling between the membrane and the component requires a small quantity of water or couplant. The conformable wedge combines the acoustic performance of immersion technique with good coupling and low attenuation.
>

NDTkit RT

NDTkit RT, TESTIA's Digital Radiography software The NDTkit product line software for X-ray analysi
...
s. NDTkit RT is a software benefiting from the Ultis kernel which is dedicated to radiographic image analysis. It offers a set of tools and filtering processes to assist RT operators in finding relevant flaws.
>

EKOSCAN Phased Array

In order to always fit your needs, EKOSCAN can manufacture any type of UT transducer, either convent
...
ional or Phased Array. As an ISO 9001: 2015 certified company, EKOSCAN is extremely careful as far a material selection and manufacturing processes are concerned. Our probes guarantee our customers the benefits of latest innovations regarding piezo-composite, backing, impedance adaptation layer, etc. Specific probes for hostile environment: high temperature, high pressure, corrosive environment,etc. Specific probes designed to fit your specific application: optimization of every parameter to guarantee you the best detection.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window