acceptance criteria of PMI

Dear Experts,
in some PMI reports i found a comment written in bottom side----the measured value of alloying elements shall be within 10 percent of the specified level------from where this tolerance has been taken? is it mentioned in code anywhere?

 
 Reply 
 
Abderrahmane Gaouas
NDT Inspector, - sgs
sgs, Algeria, Joined Jun 2010, 9

Abderrahmane Gaouas

NDT Inspector, - sgs
sgs,
Algeria,
Joined Jun 2010
9
12:34 May-12-2016
Re: acceptance criteria of PMI
In Reply to vivek at 15:13 May-09-2016 (Opening).

For acceptance criteria of PMI, it shall be demonstrated that materials contain the amount of alloying elements shown in the material specification. Alloys shall be deemed acceptable if the alloying elements are each within ten percent (10%) of the values.
Welds having consumable material content that matches, or nearly matches, the base metal composition within approximately twelve and half percent (± 12.5%) of the ranges allowed in ASME Section II, Part C for each element.
Acceptance criteria for dissimilar metal alloy welds shall be in accordance with the welding consumable material specified in the approved welding procedure. The effects of dilution between the different base metals and the filler metal shall be taken into account when determining the nominal as-deposited weld metal composition.

 
 Reply 
 

Product Spotlight

Echomac® PA Bar Tester

The Echomac® PA BT provides 100% inspection of round bars for core and surface defects, at speeds u
...
p to 2 m/sec, depending on the specific application. The unit allows producers to handle a much larger range of diameters in one installation, and is available in 3 models to test 10 – 75mm diameter (small model); 20 – 130mm (medium model) or 50 – 254mm (large model) bars.
>

FD800 Bench Top Flaw Detectors

The bench-top FD800 flaw detector range combines state-of-the-art flaw detection with advanced mater
...
ial thickness capabilities. Designed for use in the laboratory these gauges are the tool you need for all your flaw detecting needs.
>

Ultrasonic Probe Recharacterization Service

NDT Systems offers a comprehensive Aftercare and Recharacterization Service for all our ultrasonic
...
probes. The Recharacterization Service is fully compliant with International ASTM E1065 Standard Guide (and other applicable standards) and offers complete documentation, traceable to the ASTM E1065 Standard. For more details or to schedule Recharacterization Services contact ndtsales@ndtsystems.com
>

Robotic laser shearography enables 100% inspection of complex, flight-critical composite structures

An article in “Composites World Magazine” showcases Non Destructive Testing of aero-structures
...
with Laser Shearography. Over the years Dantec Dynamics has supplied many solutions for the aerospace industry. Referring to specific customer projects several of these cases are examined to outline the advantages of using Laser Shearography for automated defect detection.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window