Surface indication after MPI
zoom image



Dear All,

Refer to image.Few LW joint show this indication after MPI.Very clear line of indication at weld toe.But what make me confuse is after perform RT and UT , no indication or defect was detected.After do grinding and re-mpi, the indicatiom still occur.Expected this is cold lap.Material is carbon steel,double V welding and SAW welding process.Hope some kniw about this can explain to me.Very appreciated for the help.Thanks.

 
 Reply 
 
ezio
Other, Retired ex Laboratory Technical Manager
OMECO Research Centre, Italy, Joined Sep 2008, 278

ezio

Other, Retired ex Laboratory Technical Manager
OMECO Research Centre,
Italy,
Joined Sep 2008
278
14:44 Apr-03-2018
Re: Surface indication after MPI
In Reply to Huzairi at 11:57 Apr-03-2018 (Opening).

Hello Huzairi, differenza di permeabilità magnetica tra materiale base e materiale di apporto?

 
 Reply 
 
P V SASTRY
R & D, NDT tecniques metallurgy
TAKEN VRS FROM THE POSITION OF SR. DEPUTY GENERAL MANAGER BHEL CORPORATE R&D, India, Joined Jan 2003, 195

P V SASTRY

R & D, NDT tecniques metallurgy
TAKEN VRS FROM THE POSITION OF SR. DEPUTY GENERAL MANAGER BHEL CORPORATE R&D,
India,
Joined Jan 2003
195
14:46 Apr-03-2018
Re: Surface indication after MPI
In Reply to Huzairi at 11:57 Apr-03-2018 (Opening).


These indications are most probably due to permeability changes between the weld and parent metal.

Whenever such indications are encountered first PT has to be done (later may be RT and UT).

Please do PT and if there are no significant indications you can clear the joint.

However the indications are much sharper than normal. Hope you are going to give a proper thermal treatment like SR.

Best Wishes

P V SASTRY

 
 Reply 
 

Product Spotlight

NDT.net launches mobile-friendly design

NDT.net has revamped its website providing a mobile-friendly design.The front page received a comp
...
letely new design and all other sections are now reacting responsively on mobile devices. This has been a major step to make our website more user- friendly.
>

Ultrasonic Testing Immersion Tanks with Unmatched Scanning Features

TecScan’s non-destructive testing Ultrasonic Immersion Tanks & scanners are designed for high pe
...
rformance and demanding NDT testing applications. Our Scan3D™ line of High Precision Immersion Tanks are specifically designed for automated ultrasonic testing of complex composites parts used in aerospace and industrial applications.
>

IntraPhase Athena Phased Array System

The Athena Phased Array system, manufactured by WesDyne NDE Products & Technology, consists of a pha
...
sed array acquisition system and PC running IntraSpect software. A PC is used to perform acquisition, analysis and storage of the data. System hardware is capable of operating up to four data sets with any combination of phased array or conventional UT probes. NOW AVAILABLE IN 64-64 CONFIGURATION.
>

On Demand Webinar: Improve the Efficiency and Accuracy of Inspection Scanning

On-demand webinar on scanning technology that helps improve the efficiency and accuracy of ultrasoni
...
c inspections in oil and gas, aerospace, manufacturing and other industrial applications. The webinar features a scanning solution for multiple inspection environments, including flat and curved specimens, magnetic and nonmagnetic surfaces and raster scanning over long distances. View it today.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window