UT QUESTION

When using a focused, straight beam search unit for lamination scanning in an immersion test of a steel plate, a change in water path of 0.2 in, will result in the focal point moving in the steel a distance of?
Pls provide steps and answer, thanks.

 
 Reply 
 
Ed Ginzel
R & D, -
Materials Research Institute, Canada, Joined Nov 1998, 1300

Ed Ginzel

R & D, -
Materials Research Institute,
Canada,
Joined Nov 1998
1300
19:49 Jun-24-2018
Re: UT QUESTION
In Reply to XIAO WEI at 17:00 Jun-24-2018 (Opening).

This sounds like a classroom assignment question. Odd you should ask about a 0.2 inch change.
I do not recall the imperial units being used in Singapore when I visited some years ago. In fact, we read that the official conversion to metric occurred in 1981 in Singapore.
Instead of others working through the step by step equations for you, I suggest you go to the ultrasonic basics seen in Technical Notes (https://mbi-ctac.sites.medinfo.ufl.edu/files/2017/02/ultrasound-basics.pdf) and solve for yourself the equation #13 on page 45.

 
 Reply 
 
Anmol Birring
Consultant,
Birring NDE Center, Inc., USA, Joined Aug 2011, 805

Anmol Birring

Consultant,
Birring NDE Center, Inc.,
USA,
Joined Aug 2011
805
22:19 Jun-24-2018
Re: UT QUESTION
In Reply to XIAO WEI at 17:00 Jun-24-2018 (Opening).

0.05 inch

 
 Reply 
 
ASHOK KUMAR PATRA
,
Saudi K-KEM Engineering service co, Saudi Arabia, Joined May 2018, 55

ASHOK KUMAR PATRA

,
Saudi K-KEM Engineering service co,
Saudi Arabia,
Joined May 2018
55
15:23 Jun-25-2018
Re: UT QUESTION
In Reply to XIAO WEI at 17:00 Jun-24-2018 (Opening).

0.2/4=0.05 inch Ans

 
 Reply 
 
Xiao Wei
Engineering,
UniSA, Singapore, Joined Jun 2018, 10

Xiao Wei

Engineering,
UniSA,
Singapore,
Joined Jun 2018
10
15:45 Jun-25-2018
Re: UT QUESTION
In Reply to ASHOK KUMAR PATRA at 15:23 Jun-25-2018 .

Hi Ashok, where does 4 come from?

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 889

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
889
21:26 Jun-25-2018
Re: UT QUESTION
In Reply to Ed Ginzel at 19:49 Jun-24-2018 .

Ed, I bow to you my friend. You are a wise teacher.

To bad our young technicians do not see the value of such exercise. The Orient has changed very much.

 
 Reply 
 
ASHOK KUMAR PATRA
,
Saudi K-KEM Engineering service co, Saudi Arabia, Joined May 2018, 55

ASHOK KUMAR PATRA

,
Saudi K-KEM Engineering service co,
Saudi Arabia,
Joined May 2018
55
10:23 Jun-27-2018
Re: UT QUESTION
In Reply to Xiao Wei at 15:45 Jun-25-2018 .

The velocity of sound in steel /velocity of sound in water= 4

 
 Reply 
 
Xiao Wei
Engineering,
UniSA, Singapore, Joined Jun 2018, 10

Xiao Wei

Engineering,
UniSA,
Singapore,
Joined Jun 2018
10
17:08 Jun-27-2018
Re: UT QUESTION
In Reply to ASHOK KUMAR PATRA at 10:23 Jun-27-2018 .

Ashok, thanks, I use formula that Ed referred to calculate, result is same to yours. 0.2/(Ctm/Cw)

 
 Reply 
 

Product Spotlight

Micro CT

nanoVoxel series has nano-scale resolution by using high voltage X-ray source (from 80-300 kV) wit
...
h micro focal spot and highly sensitive detector including different kinds of big size panel detectors and lens coupling CCD.
>

Eddy Current inspection : RotoETscan Rotating Head

The rotating head RotoETscan detects the presence of longitudinal surface or sub surface defects a
...
t high speed. The rotating head is often installed directly on the production line. It is generally dedicated to the control of long products such as tubes, bars and wires, made of ferrous or non-ferrous material. It can also be used for inspection of small parts (billets).
>

NEW - TD Focus-ScanRX

The NEW Next Generation Advanced UT platform, TD Focus ScanRX - Also available as a card stack solut
...
ion. Key Improvements 1. Data acquisition is significantly faster than current design 2. Better aesthetic – closely aligns with HandyScan RX 3. Improved IP rating (Target IP66) 4. Ruggedized housing 5. Connectors are protected from impact and ingress 6. Integrated stand and separate retractable handle easy to keep clean) 7. Touchscreen with ruggedized display glass 8. 3-Axis encoder input
>

Magnetic X-Ray Pipeline Crawler 6''-60''

Suitable to work in 6''-60''diameter with speed of up to 18m/min, Max. moving diatance 5 kilometer
...
s and provide the efficient inspection of the pipeline.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window