Fred Raco, Jr.
Consultant,
RNDT, Inc., USA, Joined Jul 2002, 24

Fred Raco, Jr.

Consultant,
RNDT, Inc.,
USA,
Joined Jul 2002
24
05:06 Apr-22-2005
super austenitic plate material

Can anyone assist us on a way of measuring the residual magnetism (if any) on a super austenitic plate material after welding?


 
 Reply 
 
DJ Kallhof
DJ Kallhof
01:26 Apr-22-2005
Re: super austenitic plate material
Austenitic stainless steels unlike Martensitic don't typically have residual magnetism problems. To verify this I would suggest using a Hall Effect Probe. Just out of curiousity, what is the AMS number of the material you are dealing with?
----------- Start Original Message -----------
: Can anyone assist us on a way of measuring the residual magnetism (if any) on a super austenitic plate material after welding?
------------ End Original Message ------------




 
 Reply 
 
Jim Knowles
Jim Knowles
02:54 Apr-28-2005
Re: super austenitic plate material
Austenitics do suffer from a magnetic effect especially after a weld repair, its called retained Delta ferrite.
Too higher delta ferrite can impair the corrosion properties of the stainless material. The delta ferrite levels usually found after welding to an approved weld procedure can be between 3-6% Fe, on repairs to a repair or un authorised re running of weld cap profiles levels of Fe can rise to around 10-12%.
Equipmemt used to measure accurately is the Forster Mangnetoscop 1.068 model.


----- Start Original Message -----------
: Austenitic stainless steels unlike Martensitic don't typically have residual magnetism problems. To verify this I would suggest using a Hall Effect Probe. Just out of curiousity, what is the AMS number of the material you are dealing with?
: : Can anyone assist us on a way of measuring the residual magnetism (if any) on a super austenitic plate material after welding?
------------ End Original Message ------------




 
 Reply 
 

Product Spotlight

Compact NDT inspection-heads for measurements with active thermography

The compact inspection head is suitable for thermographic ndt tasks. The uncooled infrared camera
...
is specially developed for NDI-tasks and offers a thermal sensitivity until now known only from thermal imagers with cooled detector. All required components and functions are integrated into the inspection-head. You will only need an ethernet cable to connect the sensor with the evaluation system.
>

GUL QSR1® Scanning

How do you measure pipe wall thickness without direct access to the area? QSR® Scanning - Guide Wav
...
e Quantitative Short Range Scanning.
>

Eddy Current inspection : RotoETscan Rotating Head

The rotating head RotoETscan detects the presence of longitudinal surface or sub surface defects a
...
t high speed. The rotating head is often installed directly on the production line. It is generally dedicated to the control of long products such as tubes, bars and wires, made of ferrous or non-ferrous material. It can also be used for inspection of small parts (billets).
>

NEOS III

NEOS III is Logos Imagings lightest DR system. With a built-in battery and internal wireless commu
...
nication, the NEOS III is perfect for users that want to quickly assess an item.
>