COATING THICKNESS MEASUREMENT INSIDE COILED TUBING.N

We make carbon steel coiled tubing. Someone has sated he can coat it internally with a plastic layer 0.020 in thick. Does anyone have a device that can run 10,000 ft through coiled tubing on a spool and determine the coating thickness. It ought to be possible with eddy current stand-off sensors mounted in a 'pig" , with a lot of electronics to store the data.

Roderic K Stanley

Sr Research Scientist.


 
 Reply 
 
Leon Vandervalk
R & D
DeFelsko Corporation, USA, Joined Oct 1999, 3

Leon Vandervalk

R & D
DeFelsko Corporation,
USA,
Joined Oct 1999
3
00:16 Aug-20-1999
Re: COATING THICKNESS MEASUREMENT INSIDE COILED TUBING.N
We make handheld battery operated coating thickness gages that could easly be mounted on a pig. On board memory could easily support 10,000+ readings.


 
 Reply 
 
Leon Vandervalk
R & D
DeFelsko Corporation, USA, Joined Oct 1999, 3

Leon Vandervalk

R & D
DeFelsko Corporation,
USA,
Joined Oct 1999
3
00:23 Aug-20-1999
Re: COATING THICKNESS MEASUREMENT INSIDE COILED TUBING.N
We make handheld battery operated coating thickness gages that could easily be mounted on a pig. On board memory could easily support 10,000+ readings.


 
 Reply 
 
Richard D. Roberts
Engineering, Executive Managment
Quest Integrity Group, USA, Joined Nov 1998, 78

Richard D. Roberts

Engineering, Executive Managment
Quest Integrity Group,
USA,
Joined Nov 1998
78
07:53 Sep-07-1999
Re: COATING THICKNESS MEASUREMENT INSIDE COILED TUBING.N
Dear Mr. Roderic K Stanley,

QUEST Integrated, Inc. manafactures several types of Tube ID Inspection systems. One remote pigging system inparticular utilizes both ultasonics and laser. I think it is much too large for your tubing. Can you provide more detailed specifications on the tubing (ie Diameter, Thickness, Material, etc.)?

Regards,
Richard D. Roberts
QUEST Integrated, Inc.



 
 Reply 
 

Product Spotlight

MIZ®-21C: Truly Affordable Eddy Current Handheld with Surface Array Capability

Introducing MIZ-21C, the first truly affordable handheld eddy current instrument with surface array
...
capabilities. MIZ-21C can deliver fast, accurate inspections in demanding NDT applications including aerospace, oil and gas, manufacturing, and power generation. The surface array solution can reduce inspection time by up to 95% compared to traditional handheld pencil probes. The ergonomic design, long battery life, and intuitive touchscreen mean you can inspect more areas faster than ever without fatigue.
>

NOVO Armor 15 & NOVO Armor 22

The Armor Kit Contains the NOVO Armor, which provides additional mechanical protection to the NOVO 1
...
5WN & NOVO 22WN Detectors, the Armor Stand and a traveling soft cover. - Newest shock absorbent technology case - Water resistant design - Supports wired & wireless communication - Multiple positioning options - Tripod connection using the Built-in 1/4” threads - Simple Detector battery replacement
>

FMC/TFM

Next generation for Phased Array UT is here now with FMC/TFM! Have higher resolution imaging, impr
...
oved signal to noise ratio, characterize, size and analyze defects better with access to several wave mode views and save raw FMC data for higher quality analysis.  Some of the benefits are:
  • Beautiful Image! Easier to understand what you're looking at
  • Completely focused in entire image or volume
  • Much easier to define setups before inspection
  • Easier to decipher geometry echoes from real defects
  • Oriented defects (e.g. cracks) are imaged better
  • See image from different wave modes from one FMC inspection
  • FMC data can be reprocessed/analyzed without going back to the field
>

HARDNESS TESTER TKM-459CE combi

TKM-459CE combi applies 2 methods of hardness control: UCI and Leeb. It provides high-accuracy tes
...
ting of metals and alloys as well as items of different sizes and configurations, their hardened layers and galvanic coatings. Device represents results in HB, HRC, HV and others. Shock-, dust- and water-proof housing with intuitive software make this gauge easy to use in all working conditions.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window