TOFD 190mm thickness!

Hey! Hello!
Anybody here have already inspected a weld with 190mm thickness using TOFD technique? What is the appropriate configuration?? Probes frequency, how many probes, and so on...
Thank you!



 
 Reply 
 
John
John
02:39 Dec-01-2006
Re: TOFD 190mm thickness!
I think maybe you need divide 190mm into three zones,upper 10mm can use 10MHz,zone from 10mm to 50mm can use 5MHz,and the residual zone can use 2.25MHz.
Maybe Ed Ginzel can give us some advise about this project or correct me!

----------- Start Original Message -----------
: Hey! Hello!
: Anybody here have already inspected a weld with 190mm thickness using TOFD technique? What is the appropriate configuration?? Probes frequency, how many probes, and so on...
: Thank you!
------------ End Original Message ------------




 
 Reply 
 
Udo Schlengermann
Consultant, -
Standards Consulting, Germany, Joined Nov 1998, 180

Udo Schlengermann

Consultant, -
Standards Consulting,
Germany,
Joined Nov 1998
180
00:33 Dec-04-2006
Re: TOFD 190mm thickness!
Hello,

Perhaps you can follow existing standards:

European Technical Specification
CEN/TS 14751:2004
Welding - Use of time-of-flight diffraction technique (TOFD) for examination of welds

gives detailed recommendations for butt weld thickness up to 300 mm.
E.g. for thickness between 100 mm and 200 mm: (at least) 3 depth zones 60 mm, 60 mm to 125 mm, 125 mm to 190 mm.
Test frequencies between 5 MHz and 2 MHz, depending on material properties.

Kind regards

Udo Schlengermann
GE Inspection Technologies GmbH
Huerth, Germany

----------- Start Original Message -----------
: I think maybe you need divide 190mm into three zones,upper 10mm can use 10MHz,zone from 10mm to 50mm can use 5MHz,and the residual zone can use 2.25MHz.
: Maybe Ed Ginzel can give us some advise about this project or correct me!
: : Hey! Hello!
: : Anybody here have already inspected a weld with 190mm thickness using TOFD technique? What is the appropriate configuration?? Probes frequency, how many probes, and so on...
: : Thank you!
------------ End Original Message ------------




 
 Reply 
 

Product Spotlight

FMC/TFM

Next generation for Phased Array UT is here now with FMC/TFM! Have higher resolution imaging, impr
...
oved signal to noise ratio, characterize, size and analyze defects better with access to several wave mode views and save raw FMC data for higher quality analysis.  Some of the benefits are:
  • Beautiful Image! Easier to understand what you're looking at
  • Completely focused in entire image or volume
  • Much easier to define setups before inspection
  • Easier to decipher geometry echoes from real defects
  • Oriented defects (e.g. cracks) are imaged better
  • See image from different wave modes from one FMC inspection
  • FMC data can be reprocessed/analyzed without going back to the field
>

Robotic laser shearography enables 100% inspection of complex, flight-critical composite structures

An article in “Composites World Magazine” showcases Non Destructive Testing of aero-structures
...
with Laser Shearography. Over the years Dantec Dynamics has supplied many solutions for the aerospace industry. Referring to specific customer projects several of these cases are examined to outline the advantages of using Laser Shearography for automated defect detection.
>

OmniScan™ X3 flaw detector

The OmniScan X3 flaw detector is a complete phased array toolbox. Powerful tools, like total focus
...
ing method (TFM) images and advanced visualization capabilities, enable you to complete your inspection with greater confidence.
>

AMIGO2

TSC Amigo2 - ACFM technology has developed a solid reputation for accurately detecting and sizing
...
surface-breaking cracks through paint and coatings. As the industry demands increased performance in speed, signal quality, and portability, it’s time for an evolution. It’s time for Amigo2.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window