William B. Streett
William B. Streett
08:18 Feb-12-1998
Re: Reply to the article of M. Sansalone and W. B. Street
I will begin by quoting from the first page of Chapter 18 in the book,
'Impact-Echo: Nondestructive Evaluation of Concrete and Masonry' by
Sansalone and Streett. The title of this chapter is, 'Bonded
Post-Tensioning Tendons'.

_____________________________________
'The impact-echo method can be used to detect voids in grouted tendon
ducts in many, but not all, situations. The method’s applicability depends
on the geometry of a structure and the locations and arrangement of tendon
ducts. Just as is the case for other types of flaws, small voids in tendon
ducts can be located too deeply within a structure to be detected. In some
cases, complicated arrangement of multiple ducts, such as often occur in
the flanges of concrete I-beams, can preclude detection of voids in some or
all of the ducts. In other cases, portions of structures can be
successfully tested and information can be gained that permits an engineer
to draw conclusions about the condition of the grouting along the length of
the duct. In all cases, the impact-echo method is restricted to situations
where the walls of the ducts are metal rather than plastic.'
'Effective use of the impact-echo method for detecting voids in
grouted tendon ducts requires knowledge of the location of the ducts within
the structure. This information is typically obtained from plans and/or the
use of magnetic or eddy-current cover meters to locate the centerlines of
the metal ducts. Once the duct locations are known, impact-echo tests can
be performed to search for voids.'
_____________________________________________

Mr Krause describes a structure that is 600 x 2000 x 1500 mm. For
impact-echo this is a bounded structure that will respond with many modes
of cross-sectional vibration, and the resulting waveform and spectrum will
be complex and difficult to interpret. No one who understands the
capabilities and limitations of impact-echo would attempt to locate flaws
in a structure of this shape without first performing extensive
3-dimensional, finite-element, computer simulations to obtain detailed
information about the response of the solid structure. Mr. Krause states
that computer simulations were performed for his specimen, but no details
are given. The only computer simulations we know to be successful for a
case such as this are those described by Sansalone et al. in references
[39, 40, 41] in http://www.ndt.net/article/0298/streett/refer.htm
Even with information from computer simulations it is unlikely that
impact-echo signals from flaws at the mid-point of the 600mm dimension in
a 600 x 1500 x 2000mm structures can be separated from the cross-sectional
mode signals. It has been made very clear in published papers on the
impact-echo method that structures bounded in 2 dimensions, such as beams
and columns, respond differently from plate structures, which are defined
as structures in which the lateral dimensions are at lease five times
greater than the thickness. The impact-echo response of beams and columns
is discussed at length in Chapters 21 and 22 in the book by Sansalone and
Streett: http://www.impact-echo.com/Impact-Echo/bullbrie.htm

A 600mm thick slab that has lateral dimensions greater than 3 or 4 meters
will respond to impact-echo tests as a plate, and it will be a
straightforward matter to locate many types of flaws. However, a
post-tensioning duct located at a depth of 300mm (one-half of the
thickness) presents a special case. Multiple P-wave reflections from the
steel in a fully grouted duct will have the same frequency the P-wave
reflections from the bottom of the plate, and it will not be possible to
identify the response from the fully grouted duct. It will, however, be
possible to identify a void in the duct. For ducts that are located well
above the middle point of the thickness, both grouted and ungrouted ducts
can be detected. This is explained in Chapter 18 of the book by Sansalone
and Streett. If the ducts are located very close to the bottom of the
plate, they may be too deep to be detected. In Chapter 9 of Sansalone and
Streett it is pointed out that flaws with lateral dimensions less than
about one-fourth of their depth cannot be detected. A 100mm wide flaw at a
depth of 450mm, in a 600mm thick plate, cannot be detected. If the opposite
side of the plate is accessible, where the depth is 50mm to 100mm, the flaw
can easily be detected.

If the post-tensioned structure to be tested is a portion of a beam or
column, such as the web of an I-beam, then locating voids in grouted tendon
ducts will be straightforward only if the dimensions of the web are such
that it behaves as a plate for impact-echo purposes. This was exactly the
case in the testing the beams of a large highway bridge in the northeastern
United States in 1995. The webs of these beams were 200mm thick and the
lateral dimensions were 2 meters or more. The post-tensioning ducts were 70
to 80mm beneath the surface. After preliminary impact-echo tests, which
identified both ungrouted and fully grouted regions in the ducts, several
ducts were opened using a jackhammer, and the impact-echo predictions were
found to be 100% accurate. Photographs of the bridge and of the opened
sections of the post-tensioning ducts can be found in the published papers
on this project, and in Chapter 18 of the book by Sansalone and Streett.
The published papers are references [11,12] in
http://www.ndt.net/article/0298/streett/refer.htm

In summary, I wish to point out that in the article on impact-echo in this
month’s on-line journal, Sansalone and Streett have said that impact-echo
can be used to locate voids in grouted tendon ducts in MANY TYPES of
post-tensioned structures. It has never been claimed that it will be
successful for all post-tensioned structures. The inability of impact-echo
to locate voids in the ducts in the specimen tested by Mr. Krause and
others is very predictable, and it is regrettable that others may have made
the claim, in advance, that impact-echo would be successful in this case.
However, it would be wrong to generalize from Mr. Krause’s experience, and
conclude that impact-echo cannot locate voids in the tendon ducts of any
post-tensioned structure. Those who wish to understand the capabilities and
limitations of impact-echo in detecting voids in the grouted tendon ducts
of post-tensioned structures should read the book and the published papers
cited above.

In answer to Mr. Krause’s question about the effects of steel reinforcing
bars on impact-echo tests, I refer those who are interested to Chapter 17
in the book by Sansalone and Streett. The short answer is that impact-echo
is not a suitable method for LOCATING reinforcing bars. By choosing the
proper diameter of the sphere used to make an impact, it is usually
possible to minimize the impact-echo response of the bars, as long as they
are bonded to the concrete, and this makes it possible to focus on other
problems. Cracking caused by corrosion of steel reinforcing bars, and the
resulting deterioration of the surrounding concrete is easily detected. A
project which saved more than $5 million in repair costs in a California
sea wall was concerned with exactly this problem. A report on this project
by the U.S. Federal Highway Administration can be found on the web at
http://www.ota.fhwa.dot.gov/roadsvr/CS011.htm. Additional details,
including photographs, can be found in Chapter 17 of Sansalone and Streett.

These discussions reinforce the point made by Dr. Grosse, that impact-echo
is not in a 'plug and play' state of development. Inflated claims have been
made for its performance, and some scientists and engineers who have used
it have spent little time studying the physics and mathematics of the
method, and examining reports of its successful use. Those who have taken
the time to learn the capabilities and limitations of the method have found
it to be useful.


Prof./Dr. William B. Streett
Cornell University
Ithaca, New York
12 February 1998




 
 Reply 
 

Product Spotlight

A1525 SOLO

A1525 Solo – the most compact and affordable TMF unit with two phased array transducers and 3D v
...
isualization and analysis software in standard delivery set. A compact, ergonomic and easy to handheld Phased Array unit based on Total Focusing Method for easy-going imaging of inspection objects with two-dimensional and three-dimensional visualization and evaluation of inspection results.
>

Teletest Focus+

Teletest Focus+ electronics have superior capabilities than rivals on the market. Beyond the usual
...
test features, Focus+ has 24 transmit channels and 24 receive channels, with an additional on-board switching capabilities. The instrument's frequency range is 10–300 kHz.
>

Eddy Current inspection : RotoETscan Rotating Head

The rotating head RotoETscan detects the presence of longitudinal surface or sub surface defects a
...
t high speed. The rotating head is often installed directly on the production line. It is generally dedicated to the control of long products such as tubes, bars and wires, made of ferrous or non-ferrous material. It can also be used for inspection of small parts (billets).
>

FD800 Bench Top Flaw Detectors

The bench-top FD800 flaw detector range combines state-of-the-art flaw detection with advanced mater
...
ial thickness capabilities. Designed for use in the laboratory these gauges are the tool you need for all your flaw detecting needs.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window