Steel - Rubber debond testing method?

I am looking for a methodology that is capable of detecting bonding/adhesive failures between a rubber type compound and heavy steel plating, and determine if off-the-shelf testing equipment is available.
The steel-side surface is mostly inaccessible. Testing must either be done from the rubber surface, or from very limited locations on the steel-side surface.
The rubber compound is approximately 2" thick and cannot be penetrated by ultrasound, at any frequency.
Critical size of debond has not been determined.

Thank you,
B Johnson
NDT Engineering
General Dynamics, Electric Boat


 
 Reply 
 
joerg collrep
Director, - Sales NDT
Dantec Dynamics GmbH, Germany, Joined Jan 2006, 4

joerg collrep

Director, - Sales NDT
Dantec Dynamics GmbH,
Germany,
Joined Jan 2006
4
08:32 Apr-05-2007
Re: Steel - Rubber debond testing method?
you should try shearography which has proved to detect easily voids inside rubber. we load your part with vacuum and the defect expands to the surface. if you need more info pls let me know or visit our homepage. best regards joerg----------- Start Original Message -----------
: I am looking for a methodology that is capable of detecting bonding/adhesive failures between a rubber type compound and heavy steel plating, and determine if off-the-shelf testing equipment is available.
: The steel-side surface is mostly inaccessible. Testing must either be done from the rubber surface, or from very limited locations on the steel-side surface.
: The rubber compound is approximately 2" thick and cannot be penetrated by ultrasound, at any frequency.
: Critical size of debond has not been determined.
: Thank you,
: B Johnson
: NDT Engineering
: General Dynamics, Electric Boat
------------ End Original Message ------------




 
 Reply 
 
Tom Nelligan
Engineering,
retired, USA, Joined Nov 1998, 390

Tom Nelligan

Engineering,
retired,
USA,
Joined Nov 1998
390
01:14 Apr-05-2007
Re: Steel - Rubber debond testing method?
In other situations where the rubber is thinner and more transmissive to ultrasound, we usually recommend a phase shift test using any common flaw detector and an appropriate transducer, but you indicate that won't work here due to extreme attenuation. Alternately, if testing from the points where you do have access to the steel is useful, it should be possible to evaluate the steel/rubber bond from the steel side using the ringdown technique described in the attached application note.

----------- Start Original Message -----------
: I am looking for a methodology that is capable of detecting bonding/adhesive failures between a rubber type compound and heavy steel plating, and determine if off-the-shelf testing equipment is available.
: The steel-side surface is mostly inaccessible. Testing must either be done from the rubber surface, or from very limited locations on the steel-side surface.
: The rubber compound is approximately 2" thick and cannot be penetrated by ultrasound, at any frequency.
: Critical size of debond has not been determined.
: Thank you,
: B Johnson
: NDT Engineering
: General Dynamics, Electric Boat
------------ End Original Message ------------




 
 Reply 
 
Thomas F. Murphy
Thomas F. Murphy
07:15 Apr-06-2007
Re: Steel - Rubber debond testing method?
Hello all,

My employer, GE Inspection has a system used for this application in rubber covered rolls. It operates by the principle of heating the metal from the rubber, inductively, and monitoring the transferred heat to the rubber. Lack of thermal transfer indicates a lack of bond. If you are interested in it I will give you the correct contacts for further information.

Kind regards all,
Tom

Kindest regards,
Tom




 
 Reply 
 
Trevor Easton
Engineering
Dofasco Inc, Canada, Joined Nov 1998, 13

Trevor Easton

Engineering
Dofasco Inc,
Canada,
Joined Nov 1998
13
04:53 Apr-13-2007
Re: Steel - Rubber debond testing method?
You might try a sub sonic method. Determine the natural frequency of a bonded portion of the rubber using a shaker. Then measure the natural frequency of a debonded portion. If there is a significant difference then a scan of the surface to measure the frequency response will provide an indication of debonding. You will of course have to develop your own transducer but it shouldn't be to difficult to adapt a small electric motor with offset mass and an accelerometer into a simple hand held monitor. Maybe a roller ball to ease the job of scanning across large areas. Perhaps an electro magnet driven at the appropriate frequency(s) the variation in its behaviour over bonded and unbonded rubber indicating areas of concern.

----------- Start Original Message -----------
: I am looking for a methodology that is capable of detecting bonding/adhesive failures between a rubber type compound and heavy steel plating, and determine if off-the-shelf testing equipment is available.
: The steel-side surface is mostly inaccessible. Testing must either be done from the rubber surface, or from very limited locations on the steel-side surface.
: The rubber compound is approximately 2" thick and cannot be penetrated by ultrasound, at any frequency.
: Critical size of debond has not been determined.
: Thank you,
: B Johnson
: NDT Engineering
: General Dynamics, Electric Boat
------------ End Original Message ------------




 
 Reply 
 

Product Spotlight

Sci Aps Z-Series Portable Handheld Analysers

The world’s only handheld analyzer that measures carbon content in stainless (yes even L-grades),s
...
teels, and cast irons. Also accepted for low Si analysis for sulfidic corrosion analysis, and is widely used in the power industry for Cr analysis, for flow accelerated corrosion applications.
>

Varex Imaging Large Field of View (FOV) Digital Detector Arrays (DDAs)

A larger FOV DDA can reduce the space and volume of the X-ray inspection system on the factory floor
...
, enable faster scanning times, better throughput and better resolution images at a lower dose. Customers can also save time and money. With these benefits in mind, Varex Imaging has designed a family of large FOV detectors (4343HE, XRD 1611, 4343DX-I, 4343CT) for our industrial imaging customers.
>

Research Center IDEKO develops an ultrasonic train wheel inspection system for CAF

The Basque Research centre IK4-IDEKO has developed a state-of-the-art ultrasonic inspection system f
...
or the train wheel. This system secures a sound condition of train wheels and is thus a significant contribution to rail transport safety. The device was delivered to CAF recently and its use allows the manufacturer to become an approved supplier of rolling stock in Italy, as it meets the demanding homologation standards of this country. \\\\r\\\\n
>

Combination of Digital Image Correlation and Thermographic Measurements

The combination of measuring results from the digital image correlation (ARAMIS, DIC) and temperat
...
ure measuring data from infrared cameras permits the simultaneous analysis of the thermal and mechanical behavior of test specimens in the materials and components testing field.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window