Dave Davies
Dave Davies
03:35 Jul-24-2007
Phased Array Weld testing

Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
Weld is standard single V sub arc as welded.


 
 Reply 
 
Michael Moles †2014 *1948
, Joined ,
08:56 Jul-24-2007
Re: Phased Array Weld testing
----------- Start Original Message -----------
: Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: Weld is standard single V sub arc as welded.
------------ End Original Message ------------


We have come across similar applications before, where space is seriously limited on one side. On one occasion, there was enough space to use a smaller array on the narrow side, and adjust the phased array set-up accordingly. This is a better solution. Is it a possible option in your case?

Michael Moles



 
 Reply 
 
Dave davies
Dave davies
03:50 Jul-25-2007
Re: Phased Array Weld testing
----------- Start Original Message -----------
: : Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: : Weld is standard single V sub arc as welded.
:
: We have come across similar applications before, where space is seriously limited on one side. On one occasion, there was enough space to use a smaller array on the narrow side, and adjust the phased array set-up accordingly. This is a better solution. Is it a possible option in your case?
: Michael Moles
------------ End Original Message ------------

Michael,
Unfortunately at the moment we have very restricted access on one side, we are trying to get the forging re designed but that won't happen soon. The distance from the section change to the weld prep is 1/2 inch which is reduced depending on the weld cap width. I'm also concerned about the blind zones in TOFD and was looking at pulse echo to cover cap and root areas so need more space if we test from both sides.


 
 Reply 
 
Ed Ginzel
R & D, -
Materials Research Institute, Canada, Joined Nov 1998, 1303

Ed Ginzel

R & D, -
Materials Research Institute,
Canada,
Joined Nov 1998
1303
03:24 Jul-25-2007
Re: Phased Array Weld testing
----------- Start Original Message -----------
: : : Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: : : Weld is standard single V sub arc as welded.
: :
: : We have come across similar applications before, where space is seriously limited on one side. On one occasion, there was enough space to use a smaller array on the narrow side, and adjust the phased array set-up accordingly. This is a better solution. Is it a possible option in your case?
: : Michael Moles
: Michael,
: Unfortunately at the moment we have very restricted access on one side, we are trying to get the forging re designed but that won't happen soon. The distance from the section change to the weld prep is 1/2 inch which is reduced depending on the weld cap width. I'm also concerned about the blind zones in TOFD and was looking at pulse echo to cover cap and root areas so need more space if we test from both sides.
------------ End Original Message ------------

Dave: One side access (e.g. pipe to flange) is a fairly typical resrtiction in UT. But even with UT inspection from one side I have seen good detection of significant flaws (side-wall nonfusion) missed by RT. Last month in NDT.net there was an announcement (http://www.ndt.net/search/docs.php3?id=4531&content=1) about a new software by Eclipse Scientific that allows you to plot beam coverage of Phased Array (and standard) probes. It even allows you to select from a database of standard wedges and Probe designs to see the sort of coverage you might be able to achive from a single position.
It might be noted that if the client wants a GOOD inspection it can be improved by grinding the weld cap off (but I find that this is rarely the option selected).


 
 Reply 
 
Simon
Simon
06:40 Jul-27-2007
Re: Phased Array Weld testing
----------- Start Original Message -----------
: Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: Weld is standard single V sub arc as welded.
------------ End Original Message ------------

Contact www.zetec.com. They have devloped one s/w for few typical and critical applications using Phased Array System. You may get some answer from them.

Simon.


 
 Reply 
 
Nguyen Duy Lan
Sales, NDT Expert
Science Engineering Consultation & Services L.C.D, Vietnam, Joined Apr 2007, 2

Nguyen Duy Lan

Sales, NDT Expert
Science Engineering Consultation & Services L.C.D,
Vietnam,
Joined Apr 2007
2
02:16 Aug-01-2007
Re: Phased Array Weld testing
----------- Start Original Message -----------
: : Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: : Weld is standard single V sub arc as welded.
: Contact www.zetec.com. They have devloped one s/w for few typical and critical applications using Phased Array System. You may get some answer from them.
: Simon.
------------ End Original Message ------------

Contact Harfang Micro. at www.harfangmicro.com. The X-32 will solve your problem.

Best regards,

Lan



 
 Reply 
 
Carlos Correia
Carlos Correia
01:37 Aug-03-2007
Re: Phased Array Weld testing
I think that PA is a very good option to replace RX and resolve the access problem, but you have to take care about the focusing process. You only can be sure of the height of defects that are in the focus distance, if the defect is out the focus, you can oversize. And the focus distance is always limited to the near field related to the effective aperture .
Well ... how to know the exact defect position to produce a popper focusing process???... I think you can do first a explore scanning whit PA, if you look something, use the classic pulse echo technique to Know the sound path as good as possible, and after that do the calibration of your PA focusing at this distance if the aperture that are selected allow a near field greater than the sound path to the defect.
Eclipse Scientific and the full version of Tomoview have a ray tracing software that you can use to simulate the beam coverage but in all cases you have to take care with the beam spread.
You can also perform a TOFD with only one transducer. Check: CHARLESWORTH J., TEMPLE J. Engineering Applications of Ultrasonic Time Of Flight Diffraction

----------- Start Original Message -----------
: : : Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: : : Weld is standard single V sub arc as welded.
: :
: : We have come across similar applications before, where space is seriously limited on one side. On one occasion, there was enough space to use a smaller array on the narrow side, and adjust the phased array set-up accordingly. This is a better solution. Is it a possible option in your case?
: : Michael Moles
: Michael,
: Unfortunately at the moment we have very restricted access on one side, we are trying to get the forging re designed but that won't happen soon. The distance from the section change to the weld prep is 1/2 inch which is reduced depending on the weld cap width. I'm also concerned about the blind zones in TOFD and was looking at pulse echo to cover cap and root areas so need more space if we test from both sides.
------------ End Original Message ------------




 
 Reply 
 
David B
David B
01:17 Oct-01-2007
Re: Phased Array Weld testing
Top 2 Phased Array instruments are:
1. X-32 from Harfang Microtechniques Inc is the best PA instrument up to 32 active elements, pulse votage up to 200V and it has DAC curves.
2. Omniscan from Olympus is the sencond with 16 active elements, 70 V pulse voltage. DAC is unavailable.

----------- Start Original Message -----------
: I think that PA is a very good option to replace RX and resolve the access problem, but you have to take care about the focusing process. You only can be sure of the height of defects that are in the focus distance, if the defect is out the focus, you can oversize. And the focus distance is always limited to the near field related to the effective aperture .
: Well ... how to know the exact defect position to produce a popper focusing process???... I think you can do first a explore scanning whit PA, if you look something, use the classic pulse echo technique to Know the sound path as good as possible, and after that do the calibration of your PA focusing at this distance if the aperture that are selected allow a near field greater than the sound path to the defect.
: Eclipse Scientific and the full version of Tomoview have a ray tracing software that you can use to simulate the beam coverage but in all cases you have to take care with the beam spread.
: You can also perform a TOFD with only one transducer. Check: CHARLESWORTH J., TEMPLE J. Engineering Applications of Ultrasonic Time Of Flight Diffraction
: : : : Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: : : : Weld is standard single V sub arc as welded.
: : :
: : : We have come across similar applications before, where space is seriously limited on one side. On one occasion, there was enough space to use a smaller array on the narrow side, and adjust the phased array set-up accordingly. This is a better solution. Is it a possible option in your case?
: : : Michael Moles
: : Michael,
: : Unfortunately at the moment we have very restricted access on one side, we are trying to get the forging re designed but that won't happen soon. The distance from the section change to the weld prep is 1/2 inch which is reduced depending on the weld cap width. I'm also concerned about the blind zones in TOFD and was looking at pulse echo to cover cap and root areas so need more space if we test from both sides.
------------ End Original Message ------------




 
 Reply 
 

Product Spotlight

Ultrasonic Testing Immersion Tanks with Unmatched Scanning Features

TecScan’s non-destructive testing Ultrasonic Immersion Tanks & scanners are designed for high pe
...
rformance and demanding NDT testing applications. Our Scan3D™ line of High Precision Immersion Tanks are specifically designed for automated ultrasonic testing of complex composites parts used in aerospace and industrial applications.
>

ISAFE3 Intrinsically Safe Sensor System

ISAFE3 intrinsically safe sensor system of Vallen Systeme is especially targeted at the petrochemica
...
l - as well as oil and gas transportation industry. The sensor system is designed for permanent monitoring or periodic inspection tasks. Sensors are available for different AE-frequency ranges optimized for corrosion and fatigue crack detection and other applications. The ISAFE 3 sensor system consists of an AE-sensor (model ISAS3) certified according to ATEX/IEC for installation in zone 0, gas group IIC, IP68, 20 to +60 °C, and a signal isolator (model SISO3) certified for installation in zone 2. An ISAS3 sensor can be mounted in atmosphere or submerged, e.g. in water or crude oil. It is supported by mounting tools for temporary (magnets) or permanent (welded) installation. ISAFE3 supports automatic sensor coupling test and can be used with any AE signal processor supporting 28V supply at 90 mA peak, e.g. Vallen Systeme ASIP-2/A.
>

Cygnus 6+ PRO Multi-Mode Ultrasonic Thickness Gauge

The Cygnus 6+ PRO thickness gauge is the most advance gauge within the Cygnus range with key featu
...
res including: comprehensive data logging; A-scan and B-scan display; manual gain control; Bluetooth connectivity; and much more. With its unique dual display and three measuring modes (Multiple-Echo, Echo-Echo and Single-Echo), this surface thickness gauge offers maximum versatility for inspections.
>

SITEX CPSERIES

Teledyne ICM’s CPSERIES has been designed with a view to revolutionizing the handling and perfor
...
mances of portable X-Ray sets. Despite having managed to halve the weight of similar portable X-Ray generators available on the market (while continuing to provide the same power output), the SITEX CPSERIES generators feature a shutter, a laser pointer, a beryllium window, an aluminum filter and two integrated diaphragms (customized sizes are available upon request). Without compromising the robustness and reliability for which ICM products are renowned, the small size and light weight of the SITEX CPSERIES will radically change the way that you perform your RT inspections. And you will see a positive impact in terms of both quality and return on investment (ROI).
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window