Tom
Tom
09:50 Aug-14-2007
Elliptical Shots

Does anyone know a general rule of thumb as to how much of an offset you should use to radiograph a 2" joint using an elliptical exposure?


 
 Reply 
 
Dent
Consultant, NDE Manager NDELevel III/3
NDT Consultant, Canada, Joined Nov 1998, 252

Dent

Consultant, NDE Manager NDELevel III/3
NDT Consultant,
Canada,
Joined Nov 1998
252
05:10 Aug-14-2007
Re: Elliptical Shots
----------- Start Original Message -----------
: Does anyone know a general rule of thumb as to how much of an offset you should use to radiograph a 2" joint using an elliptical exposure?
------------ End Original Message ------------

15 Deg should work.


 
 Reply 
 
DJ Kallhof
DJ Kallhof
08:38 Aug-14-2007
Re: Elliptical Shots
----------- Start Original Message -----------
: : Does anyone know a general rule of thumb as to how much of an offset you should use to radiograph a 2" joint using an elliptical exposure?
: 15 Deg should work.
------------ End Original Message ------------

7 : 1 ratio has worked well for me in the past. Back off 14" and offset 2" or 21" and offset 3". You get the idea. The only thing that can make it tricky is excessive weld build up of the root or crown. Take a technique and adjust accordingly.



 
 Reply 
 
chris s
chris s
00:44 Aug-15-2007
Re: Elliptical Shots
----------- Start Original Message -----------
: : : Does anyone know a general rule of thumb as to how much of an offset you should use to radiograph a 2" joint using an elliptical exposure?
: : 15 Deg should work.
: 7 : 1 ratio has worked well for me in the past. Back off 14" and offset 2" or 21" and offset 3". You get the idea. The only thing that can make it tricky is excessive weld build up of the root or crown. Take a technique and adjust accordingly.
------------ End Original Message ------------

i use the 7:1 ratio also, works fine. until you get into heavy wall


 
 Reply 
 
G.Madhesan
G.Madhesan
01:44 Aug-22-2007
Re: Elliptical Shots
As said by Mr.Dent You can use a 7:1 technique but you have to consider the thickness of the pipe because the root will vary deponds upon the wall thick.


 
 Reply 
 

Product Spotlight

Customized Probes and Transducers

With a strong development department and our own piezocomposite production, we accompany you from th
...
e first product idea to serial production. Our scientists are continuously researching new methods in the field of ultrasonic measurement technology. The progress achieved enables us to offer you optimal solutions.
>

Wireless TOFD scanner

Quick, accurate and highly reproducible welds testing. The System operates wirelessly and is compat
...
ible with any type of Windows based Laptop, Desktop or Tablet.
>

NEW - TD Focus-ScanRX

The NEW Next Generation Advanced UT platform, TD Focus ScanRX - Also available as a card stack solut
...
ion. Key Improvements 1. Data acquisition is significantly faster than current design 2. Better aesthetic – closely aligns with HandyScan RX 3. Improved IP rating (Target IP66) 4. Ruggedized housing 5. Connectors are protected from impact and ingress 6. Integrated stand and separate retractable handle easy to keep clean) 7. Touchscreen with ruggedized display glass 8. 3-Axis encoder input
>

GEKKO - Portable Phased Array Testing with TFM in Real-Time

The portable phased array testing system GEKKO provides 64 parallel test channels. On creating testi
...
ng parameters the operator is assisted by the CIVA software. Due to its modular set-up the GEKKO instrument is suitable for operators of all skill levels.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window