Elliptical Shots

Does anyone know a general rule of thumb as to how much of an offset you should use to radiograph a 2" joint using an elliptical exposure?


 
 Reply 
 
Dent
Consultant, NDE Manager NDELevel III/3
NDT Consultant, Canada, Joined Nov 1998, 252

Dent

Consultant, NDE Manager NDELevel III/3
NDT Consultant,
Canada,
Joined Nov 1998
252
05:10 Aug-14-2007
Re: Elliptical Shots
----------- Start Original Message -----------
: Does anyone know a general rule of thumb as to how much of an offset you should use to radiograph a 2" joint using an elliptical exposure?
------------ End Original Message ------------

15 Deg should work.


 
 Reply 
 
DJ Kallhof
DJ Kallhof
08:38 Aug-14-2007
Re: Elliptical Shots
----------- Start Original Message -----------
: : Does anyone know a general rule of thumb as to how much of an offset you should use to radiograph a 2" joint using an elliptical exposure?
: 15 Deg should work.
------------ End Original Message ------------

7 : 1 ratio has worked well for me in the past. Back off 14" and offset 2" or 21" and offset 3". You get the idea. The only thing that can make it tricky is excessive weld build up of the root or crown. Take a technique and adjust accordingly.



 
 Reply 
 
chris s
chris s
00:44 Aug-15-2007
Re: Elliptical Shots
----------- Start Original Message -----------
: : : Does anyone know a general rule of thumb as to how much of an offset you should use to radiograph a 2" joint using an elliptical exposure?
: : 15 Deg should work.
: 7 : 1 ratio has worked well for me in the past. Back off 14" and offset 2" or 21" and offset 3". You get the idea. The only thing that can make it tricky is excessive weld build up of the root or crown. Take a technique and adjust accordingly.
------------ End Original Message ------------

i use the 7:1 ratio also, works fine. until you get into heavy wall


 
 Reply 
 
G.Madhesan
G.Madhesan
01:44 Aug-22-2007
Re: Elliptical Shots
As said by Mr.Dent You can use a 7:1 technique but you have to consider the thickness of the pipe because the root will vary deponds upon the wall thick.


 
 Reply 
 

Product Spotlight

Immersion systems

ScanMaster ultrasonic immersion systems are designed for high throughput, multi shift operation in a
...
n industrial or lab environment. These fully integrated systems provide various scanning configurations and incorporate conventional and phased arrays technologies to support diverse applications, such as inspection of disks, bars, shafts, billets and plates. All of ScanMaster immersion systems are built from high accuracy scanning frames allowing for scanning of complex parts and include a multi-channel ultrasonic instrument with exceptional performance. The systems are approved by all major manufacturers for C-scan inspection of jet engine forged discs. Together with a comprehensive set of software modules these flexible series of systems provide the customer with the best price performance solutions.
>

Ultrasonic Testing Immersion Tanks with Unmatched Scanning Features

TecScan’s non-destructive testing Ultrasonic Immersion Tanks & scanners are designed for high pe
...
rformance and demanding NDT testing applications. Our Scan3D™ line of High Precision Immersion Tanks are specifically designed for automated ultrasonic testing of complex composites parts used in aerospace and industrial applications.
>

SITEX CPSERIES

Teledyne ICM’s CPSERIES has been designed with a view to revolutionizing the handling and perfor
...
mances of portable X-Ray sets. Despite having managed to halve the weight of similar portable X-Ray generators available on the market (while continuing to provide the same power output), the SITEX CPSERIES generators feature a shutter, a laser pointer, a beryllium window, an aluminum filter and two integrated diaphragms (customized sizes are available upon request). Without compromising the robustness and reliability for which ICM products are renowned, the small size and light weight of the SITEX CPSERIES will radically change the way that you perform your RT inspections. And you will see a positive impact in terms of both quality and return on investment (ROI).
>

NOVO Armor 15 & NOVO Armor 22

The Armor Kit Contains the NOVO Armor, which provides additional mechanical protection to the NOVO 1
...
5WN & NOVO 22WN Detectors, the Armor Stand and a traveling soft cover. - Newest shock absorbent technology case - Water resistant design - Supports wired & wireless communication - Multiple positioning options - Tripod connection using the Built-in 1/4” threads - Simple Detector battery replacement
>