08:55 Sep-07-2007
IQI/penetrameter for Exotic Material?

Hello guys..
would appreciate if u guys can assist me in determining the suitable IQI for RT on exotic material such as Hastelloy-X, Nimonic 263 and others. Is there any IQI made of these materials? can i just simply use the IQI that we use on carbon steel? Thanking u in advance!


 
 Reply 
 
DJ Kallhof
DJ Kallhof
03:25 Sep-07-2007
Re: IQI/penetrameter for Exotic Material?
----------- Start Original Message -----------
: Hello guys..
: would appreciate if u guys can assist me in determining the suitable IQI for RT on exotic material such as Hastelloy-X, Nimonic 263 and others. Is there any IQI made of these materials? can i just simply use the IQI that we use on carbon steel? Thanking u in advance!
------------ End Original Message ------------

Both Hastelloy-X and Nimonic 263 are primarily Nickel based alloys. Without knowing the code you are working to I am hesitant to state wether you are able to use anything else. However, I believe you are able to substitute a softer material, ie. Steel for Nickel, when you are in a pinch. The down side is, it will require thicker shimming of the steel to compensate for the hardness difference. Remember to select the IQI based on the material thickness you are attempting to radiograph, not on the thickness of the shim you are required to use to even out the densities.


 
 Reply 
 
ET
ET
04:19 Sep-12-2007
Re: IQI/penetrameter for Exotic Material?
----------- Start Original Message -----------
: : Hello guys..
: : would appreciate if u guys can assist me in determining the suitable IQI for RT on exotic material such as Hastelloy-X, Nimonic 263 and others. Is there any IQI made of these materials? can i just simply use the IQI that we use on carbon steel? Thanking u in advance!
: Both Hastelloy-X and Nimonic 263 are primarily Nickel based alloys. Without knowing the code you are working to I am hesitant to state wether you are able to use anything else. However, I believe you are able to substitute a softer material, ie. Steel for Nickel, when you are in a pinch. The down side is, it will require thicker shimming of the steel to compensate for the hardness difference. Remember to select the IQI based on the material thickness you are attempting to radiograph, not on the thickness of the shim you are required to use to even out the densities.
------------ End Original Message ------------

That is correct. You can use an IQI from a lower group number as defined in ASME Sec. V, basically less dense materials



 
 Reply 
 
Vishal Gupta
Vishal Gupta
15:18 Jun-16-2013
Re: IQI/penetrameter for Exotic Material?
In Reply to DJ Kallhof at 03:25 Sep-07-2007 .

For Selection of the penetrameters you can refer ASTM E-747. For Nickel based alloys contaning Ni-Cr-Mo as major elements and Ni-Cu alloys use Group-3 and group-4 penetrameter respectively.

 
 Reply 
 

Product Spotlight

NOVO Armor 15 & NOVO Armor 22

The Armor Kit Contains the NOVO Armor, which provides additional mechanical protection to the NOVO 1
...
5WN & NOVO 22WN Detectors, the Armor Stand and a traveling soft cover. - Newest shock absorbent technology case - Water resistant design - Supports wired & wireless communication - Multiple positioning options - Tripod connection using the Built-in 1/4” threads - Simple Detector battery replacement
>

Extended Range Variable Wall® Piping Calibration Blocks for Longseam Inspection

This set of two blocks has been specially designed for situations where ultrasonic examination tak
...
es place circumferentially or “around the curve” for applications such as inspection of longseam welds in piping and vessels. Jointly designed by PH Tool and Holloway NDT, the blocks feature side-drilled hole reflectors positioned within novel compound-curves, each with multiple thickness steps. The unique design results in a light and compact form factor, with the largest block weighing just over 15 lbs and spanning just 16 ¾”. Coverage is provided for nominal pipe sizes from 6” to 10” in the small block and 12” to a whopping 56” in the large block. The compound OD curves and multiple wall thicknesses actually exceed ASME requirements, providing exceptional signal response and measurement accuracy. Properly managing beam divergence off the ID and stabilizing beam skew due to probe rocking is essential to maintaining a consistent calibration when inspecting lengthwise on curved surfaces.
>

SITEX CPSERIES

Teledyne ICM’s CPSERIES has been designed with a view to revolutionizing the handling and perfor
...
mances of portable X-Ray sets. Despite having managed to halve the weight of similar portable X-Ray generators available on the market (while continuing to provide the same power output), the SITEX CPSERIES generators feature a shutter, a laser pointer, a beryllium window, an aluminum filter and two integrated diaphragms (customized sizes are available upon request). Without compromising the robustness and reliability for which ICM products are renowned, the small size and light weight of the SITEX CPSERIES will radically change the way that you perform your RT inspections. And you will see a positive impact in terms of both quality and return on investment (ROI).
>

Robotic laser shearography enables 100% inspection of complex, flight-critical composite structures

An article in “Composites World Magazine” showcases Non Destructive Testing of aero-structures
...
with Laser Shearography. Over the years Dantec Dynamics has supplied many solutions for the aerospace industry. Referring to specific customer projects several of these cases are examined to outline the advantages of using Laser Shearography for automated defect detection.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window