Phased Array Weld testing

Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
Weld is standard single V sub arc as welded.


 
 Reply 
 
Michael Moles †2014 *1948
, Joined ,
08:56 Jul-24-2007
Re: Phased Array Weld testing
----------- Start Original Message -----------
: Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: Weld is standard single V sub arc as welded.
------------ End Original Message ------------


We have come across similar applications before, where space is seriously limited on one side. On one occasion, there was enough space to use a smaller array on the narrow side, and adjust the phased array set-up accordingly. This is a better solution. Is it a possible option in your case?

Michael Moles



 
 Reply 
 
Dave davies
Dave davies
03:50 Jul-25-2007
Re: Phased Array Weld testing
----------- Start Original Message -----------
: : Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: : Weld is standard single V sub arc as welded.
:
: We have come across similar applications before, where space is seriously limited on one side. On one occasion, there was enough space to use a smaller array on the narrow side, and adjust the phased array set-up accordingly. This is a better solution. Is it a possible option in your case?
: Michael Moles
------------ End Original Message ------------

Michael,
Unfortunately at the moment we have very restricted access on one side, we are trying to get the forging re designed but that won't happen soon. The distance from the section change to the weld prep is 1/2 inch which is reduced depending on the weld cap width. I'm also concerned about the blind zones in TOFD and was looking at pulse echo to cover cap and root areas so need more space if we test from both sides.


 
 Reply 
 
Ed Ginzel
R & D, -
Materials Research Institute, Canada, Joined Nov 1998, 1303

Ed Ginzel

R & D, -
Materials Research Institute,
Canada,
Joined Nov 1998
1303
03:24 Jul-25-2007
Re: Phased Array Weld testing
----------- Start Original Message -----------
: : : Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: : : Weld is standard single V sub arc as welded.
: :
: : We have come across similar applications before, where space is seriously limited on one side. On one occasion, there was enough space to use a smaller array on the narrow side, and adjust the phased array set-up accordingly. This is a better solution. Is it a possible option in your case?
: : Michael Moles
: Michael,
: Unfortunately at the moment we have very restricted access on one side, we are trying to get the forging re designed but that won't happen soon. The distance from the section change to the weld prep is 1/2 inch which is reduced depending on the weld cap width. I'm also concerned about the blind zones in TOFD and was looking at pulse echo to cover cap and root areas so need more space if we test from both sides.
------------ End Original Message ------------

Dave: One side access (e.g. pipe to flange) is a fairly typical resrtiction in UT. But even with UT inspection from one side I have seen good detection of significant flaws (side-wall nonfusion) missed by RT. Last month in NDT.net there was an announcement (http://www.ndt.net/search/docs.php3?id=4531&content=1) about a new software by Eclipse Scientific that allows you to plot beam coverage of Phased Array (and standard) probes. It even allows you to select from a database of standard wedges and Probe designs to see the sort of coverage you might be able to achive from a single position.
It might be noted that if the client wants a GOOD inspection it can be improved by grinding the weld cap off (but I find that this is rarely the option selected).


 
 Reply 
 
Simon
Simon
06:40 Jul-27-2007
Re: Phased Array Weld testing
----------- Start Original Message -----------
: Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: Weld is standard single V sub arc as welded.
------------ End Original Message ------------

Contact www.zetec.com. They have devloped one s/w for few typical and critical applications using Phased Array System. You may get some answer from them.

Simon.


 
 Reply 
 
Nguyen Duy Lan
Sales, NDT Expert
Science Engineering Consultation & Services L.C.D, Vietnam, Joined Apr 2007, 2

Nguyen Duy Lan

Sales, NDT Expert
Science Engineering Consultation & Services L.C.D,
Vietnam,
Joined Apr 2007
2
02:16 Aug-01-2007
Re: Phased Array Weld testing
----------- Start Original Message -----------
: : Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: : Weld is standard single V sub arc as welded.
: Contact www.zetec.com. They have devloped one s/w for few typical and critical applications using Phased Array System. You may get some answer from them.
: Simon.
------------ End Original Message ------------

Contact Harfang Micro. at www.harfangmicro.com. The X-32 will solve your problem.

Best regards,

Lan



 
 Reply 
 
Carlos Correia
Carlos Correia
01:37 Aug-03-2007
Re: Phased Array Weld testing
I think that PA is a very good option to replace RX and resolve the access problem, but you have to take care about the focusing process. You only can be sure of the height of defects that are in the focus distance, if the defect is out the focus, you can oversize. And the focus distance is always limited to the near field related to the effective aperture .
Well ... how to know the exact defect position to produce a popper focusing process???... I think you can do first a explore scanning whit PA, if you look something, use the classic pulse echo technique to Know the sound path as good as possible, and after that do the calibration of your PA focusing at this distance if the aperture that are selected allow a near field greater than the sound path to the defect.
Eclipse Scientific and the full version of Tomoview have a ray tracing software that you can use to simulate the beam coverage but in all cases you have to take care with the beam spread.
You can also perform a TOFD with only one transducer. Check: CHARLESWORTH J., TEMPLE J. Engineering Applications of Ultrasonic Time Of Flight Diffraction

----------- Start Original Message -----------
: : : Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: : : Weld is standard single V sub arc as welded.
: :
: : We have come across similar applications before, where space is seriously limited on one side. On one occasion, there was enough space to use a smaller array on the narrow side, and adjust the phased array set-up accordingly. This is a better solution. Is it a possible option in your case?
: : Michael Moles
: Michael,
: Unfortunately at the moment we have very restricted access on one side, we are trying to get the forging re designed but that won't happen soon. The distance from the section change to the weld prep is 1/2 inch which is reduced depending on the weld cap width. I'm also concerned about the blind zones in TOFD and was looking at pulse echo to cover cap and root areas so need more space if we test from both sides.
------------ End Original Message ------------




 
 Reply 
 
David B
David B
01:17 Oct-01-2007
Re: Phased Array Weld testing
Top 2 Phased Array instruments are:
1. X-32 from Harfang Microtechniques Inc is the best PA instrument up to 32 active elements, pulse votage up to 200V and it has DAC curves.
2. Omniscan from Olympus is the sencond with 16 active elements, 70 V pulse voltage. DAC is unavailable.

----------- Start Original Message -----------
: I think that PA is a very good option to replace RX and resolve the access problem, but you have to take care about the focusing process. You only can be sure of the height of defects that are in the focus distance, if the defect is out the focus, you can oversize. And the focus distance is always limited to the near field related to the effective aperture .
: Well ... how to know the exact defect position to produce a popper focusing process???... I think you can do first a explore scanning whit PA, if you look something, use the classic pulse echo technique to Know the sound path as good as possible, and after that do the calibration of your PA focusing at this distance if the aperture that are selected allow a near field greater than the sound path to the defect.
: Eclipse Scientific and the full version of Tomoview have a ray tracing software that you can use to simulate the beam coverage but in all cases you have to take care with the beam spread.
: You can also perform a TOFD with only one transducer. Check: CHARLESWORTH J., TEMPLE J. Engineering Applications of Ultrasonic Time Of Flight Diffraction
: : : : Has anyone had any success with testing 20 - 50mm thick circumferential butt welds (18 - 30 inch diameter) using phased array from one side only (one side obstructed). Code is API 1104. I'm looking to replace / supplement radiography but getting conflicting advice.
: : : : Weld is standard single V sub arc as welded.
: : :
: : : We have come across similar applications before, where space is seriously limited on one side. On one occasion, there was enough space to use a smaller array on the narrow side, and adjust the phased array set-up accordingly. This is a better solution. Is it a possible option in your case?
: : : Michael Moles
: : Michael,
: : Unfortunately at the moment we have very restricted access on one side, we are trying to get the forging re designed but that won't happen soon. The distance from the section change to the weld prep is 1/2 inch which is reduced depending on the weld cap width. I'm also concerned about the blind zones in TOFD and was looking at pulse echo to cover cap and root areas so need more space if we test from both sides.
------------ End Original Message ------------




 
 Reply 
 

Product Spotlight

OmniScan™ X3 flaw detector

The OmniScan X3 flaw detector is a complete phased array toolbox. Powerful tools, like total focus
...
ing method (TFM) images and advanced visualization capabilities, enable you to complete your inspection with greater confidence.
>

GEKKO - Portable Phased Array Testing with TFM in Real-Time

The portable phased array testing system GEKKO provides 64 parallel test channels. On creating testi
...
ng parameters the operator is assisted by the CIVA software. Due to its modular set-up the GEKKO instrument is suitable for operators of all skill levels.
>

Wireless TOFD scanner

Quick, accurate and highly reproducible welds testing. The System operates wirelessly and is compat
...
ible with any type of Windows based Laptop, Desktop or Tablet.
>

OPBOX with standard software is able to do all types of inspections and measurements: flaw detection in welds and materials, scanning of objects, testing composite materials, forged and moulded pieces, many UT inspections, measurements of properties of ma

Typical applications: UT measurements with pulse technique, Measurement of thicknesses also at hig
...
h temperatures, Measurements of properties of materials, including fluids and gases We are delivering a standard version of the software (for any Microsoft Windows up to 10 x64 with Microsoft Hardware certification report Approved) and for special needs: SDK with ready to use examples for LabView, MATLAB x64, C++ wrapper for dll, Python and Linux., and also low-level description of how to control our devices directly from any USB tools
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window