930 views
Technical Discussions
Peter McKibbin
Peter McKibbin
03:52 Jan-26-2000
concrete inspection

Can anyone advise me of methods to inspect concrete lined tanks and pipes. Visual is not a problem but defects which are not readily visible are. It has been suggested that I try low freq UT

Any advise / comments appreciated


 
 Reply 
 
Joseph E. Pascente
Engineering
Lixi, Inc., USA, Joined Nov 1998, 39

Joseph E. Pascente

Engineering
Lixi, Inc.,
USA,
Joined Nov 1998
39
00:25 Jan-27-2000
Re: Concrete Inspection
The Lixi Profiler will find defects of concrete lined pipes. The results from this technology is density measurement of the total concrete and the steel of the pipe.


 
 Reply 
 
Jens Forker
Jens Forker
07:10 Jan-27-2000
Re: concrete inspection

: Can anyone advise me of methods to inspect concrete lined tanks and pipes. Visual is not a problem but defects which are not readily visible are. It has been suggested that I try low freq UT

<



 
 Reply 
 
John O'Brien
Consultant, -
Chevron ETC , USA, Joined Jan 2000, 280

John O'Brien

Consultant, -
Chevron ETC ,
USA,
Joined Jan 2000
280
03:00 Jan-27-2000
Re: concrete inspection
It depends upon what the specific application is and the defects you are considering.

Cement Lined Carbon Steel Piping as commonly used in Firewater systems is commonly a problem with internal cement lining failing at the welded field joints in particular. Many people have had success in finding gross defects by using Infrared Imaging where there is sufficient variation in the internal process fluid and the external temperature. Areas where the cement has broken away show up warmer. It is however a quick search technique, very difficult to quantify damage with and of course you need to pipe surface to be available for inspection.

The Lixi Scope imaging device mentioned by Joe Pascent will of course also do an excellent job and the new version will provide quantification information if calibrated for the application.

Conventional ultrasonic is also commonly used from the non concrete side to look for lack of interface. It can be slow and in some case unreliable. Also is most effective when substantial deterioration has taken place.

If you wnat a more sophisticated inspection for early damage such as disbondment then probably something like the Ultraspec Ultrasonic Spectroscopy System would be best. This uses swept frequencys which can be analysed in real time and provides very good indications of back surface properties at much higher sensitivities. This should clearly show breakdown in bond interface between the base pipe and the lining material.
Concrete lined tanks depends on how much access you have to them and the extent of damage expected. If you can get to the lined side - Infrared Thermography either passive or Pulsed Wave may provide information on disbonding etc. Technique is used often in concrete decking.

If you can get access to the outside (I assume these are typically carbon steel tanks lined with cement for water slops, sewage, seawater etc. If this access is available you may be able to apply an AE test but you have to consider signal path travel , thickness of cement etc. Scanningthe surface with a Neutron Backsactter device might indicate areas of differentiation where water has seeped into structure etc.

Thats as far as my thinking goes.

Regards

John O'Brien



 
 Reply 
 

Product Spotlight

AIS229 - Multipurpose Real Time System

Latest standard & automatic real time system developed by Balteau. The AIS229 has been designed to
...
do series inspection in a wide variety of industry. Composed of a shielded cabinet, 5 axis manipulator, x-ray generator and tubehead from 160kV to 225kV, a fl at panel & much more, the AIS229 is most certainly one of the most multipurpose RTR system available on the market.
>

NEW Wheel Type Phased Array Probe

DOPPLER NEW Wheel Type Phased Array Probe, more stable, new tyre makes lesser acoustic attenuation
...
, much lighter makes easier to handle, more slim size, magnetic and mechanical encoder optional etc...more
>

Sci Aps Z-Series Portable Handheld Analysers

The world’s only handheld analyzer that measures carbon content in stainless (yes even L-grades),s
...
teels, and cast irons. Also accepted for low Si analysis for sulfidic corrosion analysis, and is widely used in the power industry for Cr analysis, for flow accelerated corrosion applications.
>

ISONIC 3510

Very Powerful Superior Performance Extremely Portable Smart Phased Array Ultrasonic Flaw Detector an
...
d Recorder with 2 Conventional UT and TOFD Channels uniquely combines PA, single- and multi-channel conventional UT, and TOFD modalities providing 100% raw data recording and imaging. Suitable for all kinds of every-day ultrasonic inspections
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window