Elmar van den Elzen
Elmar van den Elzen
06:17 Jan-12-2000
magnetism in steel

Dear Sirs,

For a customer we inspect steel rolls (3% chrome) for cold rolling steel strip. In the heavily stessed zones of the roll, where the roll material has probably been deformed, magnetism is introduced. This magnetism is finely distributed and the magnetism extends at least several millimeters into the roll body.

We would like to know the cause of this effect.
- Could magnetism be introduced into steel by local deformation?
- Or is it likely that an external magnetic field can be 'frozen' into the material by deformation?

We would appreciate any help to understand this fenomenon or hear from any cases with similar effects observed.

Thank you,
Lismar Engineering,
Elmar van den Elzen



 
 Reply 
 
Jens Forker
Jens Forker
07:00 Jan-12-2000
Re: magnetism in steel
: We would like to know the cause of this effect.
: - Could magnetism be introduced into steel by local deformation?
: - Or is it likely that an external magnetic field can be 'frozen' into the material by deformation?

<<


 
 Reply 
 
Thomas David Koble
Thomas David Koble
02:39 Feb-01-2000
Re: magnetism in steel
Dear Elamr,

knowing the chrome content, I suppose that the steel is a ferromagnetic material.

It is well known that magnetostriction occures in ferromagnetic materials.
This means that the shape and length of the matrial changes if the magnetization changes and vice versa.
From my point of view this is what you are observing.

For more infromation please look for articles on:
magnetostriction, magnetomechanical effect, magnetoelastic effect
(different names for the same physical effect !)

Best regards

Dag

Thomas


: Dear Sirs,

: For a customer we inspect steel rolls (3% chrome) for cold rolling steel strip. In the heavily stessed zones of the roll, where the roll material has probably been deformed, magnetism is introduced. This magnetism is finely distributed and the magnetism extends at least several millimeters into the roll body.

: We would like to know the cause of this effect.
: - Could magnetism be introduced into steel by local deformation?
: - Or is it likelythat an external magnetic field can be 'frozen' into the material by deformation?

: We would appreciate any help to understand this fenomenon or hear from any cases with similar effects observed.

: Thank you,
: Lismar Engineering,
: Elmar van den Elzen





 
 Reply 
 

Product Spotlight

AIS229 - Multipurpose Real Time System

Latest standard & automatic real time system developed by Balteau. The AIS229 has been designed to
...
do series inspection in a wide variety of industry. Composed of a shielded cabinet, 5 axis manipulator, x-ray generator and tubehead from 160kV to 225kV, a fl at panel & much more, the AIS229 is most certainly one of the most multipurpose RTR system available on the market.
>

Echomac® PA Bar Tester

The Echomac® PA BT provides 100% inspection of round bars for core and surface defects, at speeds u
...
p to 2 m/sec, depending on the specific application. The unit allows producers to handle a much larger range of diameters in one installation, and is available in 3 models to test 10 – 75mm diameter (small model); 20 – 130mm (medium model) or 50 – 254mm (large model) bars.
>

FAAST-PA! OEM Patented phased Array for high speed UT inspection

Multiangle, Multifocus, Multifrequency, Multibeam. Instead of stacking UT electronics and having m
...
any PA probes, FAAST-PA is able to transmit all delay laws within ONE single shot in Real time.
>

Semi-Automated Phased Array Immersion System for Small Composite Parts

Turn-key semi-automated system as an improved and affordable solution for inspection of small comp
...
osite parts. Includes support table, immersion tank, scanner, PA instrument, PC, Analysis software, database, wedge management and other options.
>