Technical Discussions
jarno de jonge
jarno de jonge
06:12 Apr-01-2008
comparing UT acceptance ASME VIII, B31.1 and B31.3

Dear Colleagues,

After comparing the acceptance criteria from these 3 codes it seems like the acceptance for B31.3 is much less stringent then for the other two codes.

Is this correct and does anbody know why this is? Or am I just overlooking something in B31.3?

The acceptance for ASME VIII and B31.1 seem to be exactly the same. They don't allow linear discontinuities over 20% DAC and reject rounded discontinuities when they exceed a certain length and 100%DAC.

As far as I can find; B31.3 does not reject rounded discontinuties. And linear discontinuties are allowed to have some length and are allowed to produce indications up to 100% DAC (similar as is allowed for the rounded indications in VIII and B31.1).

Looking forward to an explanation.

Kind Regards,

Jarno de Jonge



 
 Reply 
 
bob sudharmin
Engineering, Reliability and Integrity Eng
Shell Malaysia Trading, Malaysia, Joined Jan 2008, 54

bob sudharmin

Engineering, Reliability and Integrity Eng
Shell Malaysia Trading,
Malaysia,
Joined Jan 2008
54
06:05 Apr-02-2008
Re: comparing UT acceptance ASME VIII, B31.1 and B31.3

Acceptance criteria does not necessarily be the same when comparison is being made against different code requirements.
ASME Viii is a pressure vessel code, B31.1 - Power Piping and B31.3 - Process Piping.
It is true that B31.3 is less stringent but then again take note it is a piping system designed for and above 0 but less than 105Kpa (15psi)

----------- Start Original Message -----------
: Dear Colleagues,
: After comparing the acceptance criteria from these 3 codes it seems like the acceptance for B31.3 is much less stringent then for the other two codes.
: Is this correct and does anbody know why this is? Or am I just overlooking something in B31.3?
: The acceptance for ASME VIII and B31.1 seem to be exactly the same. They don't allow linear discontinuities over 20% DAC and reject rounded discontinuities when they exceed a certain length and 100%DAC.
: As far as I can find; B31.3 does not reject rounded discontinuties. And linear discontinuties are allowed to have some length and are allowed to produce indications up to 100% DAC (similar as is allowed for the rounded indications in VIII and B31.1).
: Looking forward to an explanation.
: Kind Regards,
: Jarno de Jonge
------------ End Original Message ------------




 
 Reply 
 
Ryan Burns
Ryan Burns
00:44 Apr-03-2008
Re: comparing UT acceptance ASME VIII, B31.1 and B31.3
Quote "It is true that B31.3 is less stringent but then again take note it is a piping system designed for and above 0 but less than 105Kpa (15psi)"

Mr. Sudharmin, this is not correct. 31.3 most certanly allows for pressures above 15psi.

Regards,

RB

----------- Start Original Message -----------
:
: Acceptance criteria does not necessarily be the same when comparison is being made against different code requirements.
: ASME Viii is a pressure vessel code, B31.1 - Power Piping and B31.3 - Process Piping.
: It is true that B31.3 is less stringent but then again take note it is a piping system designed for and above 0 but less than 105Kpa (15psi)
: : Dear Colleagues,
: : After comparing the acceptance criteria from these 3 codes it seems like the acceptance for B31.3 is much less stringent then for the other two codes.
: : Is this correct and does anbody know why this is? Or am I just overlooking something in B31.3?
: : The acceptance for ASME VIII and B31.1 seem to be exactly the same. They don't allow linear discontinuities over 20% DAC and reject rounded discontinuities when they exceed a certain length and 100%DAC.
: : As far as I can find; B31.3 does not reject rounded discontinuties. And linear discontinuties are allowed to have some length and are allowed to produce indications up to 100% DAC (similar as is allowed for the rounded indications in VIII and B31.1).
: : Looking forward to an explanation.
: : Kind Regards,
: : Jarno de Jonge
------------ End Original Message ------------




 
 Reply 
 
jarno de jonge
jarno de jonge
08:43 Apr-03-2008
Re: comparing UT acceptance ASME VIII, B31.1 and B31.3
There seems to be only an exclusion in B31.3 for this pressure range under certain circumstances. This means that we are just as well talking about pressurised piping.

For this reason I found it remarkable that the acceptance is less stringent for B31.3 piping than for other pressure containing parts (vessels and B31.1 piping)

Jarno

----------- Start Original Message -----------
: Quote "It is true that B31.3 is less stringent but then again take note it is a piping system designed for and above 0 but less than 105Kpa (15psi)"
: Mr. Sudharmin, this is not correct. 31.3 most certanly allows for pressures above 15psi.
: Regards,
: RB
: :
: : Acceptance criteria does not necessarily be the same when comparison is being made against different code requirements.
: : ASME Viii is a pressure vessel code, B31.1 - Power Piping and B31.3 - Process Piping.
: : It is true that B31.3 is less stringent but then again take note it is a piping system designed for and above 0 but less than105Kpa (15psi)
: : : Dear Colleagues,
: : : After comparing the acceptance criteria from these 3 codes it seems like the acceptance for B31.3 is much less stringent then for the other two codes.
: : : Is this correct and does anbody know why this is? Or am I just overlooking something in B31.3?
: : : The acceptance for ASME VIII and B31.1 seem to be exactly the same. They don't allow linear discontinuities over 20% DAC and reject rounded discontinuities when they exceed a certain length and 100%DAC.
: : : As far as I can find; B31.3 does not reject rounded discontinuties. And linear discontinuties are allowed to have some length and are allowed to produce indications up to 100% DAC (similar as is allowed for the rounded indications in VIII and B31.1).
: : : Looking forward to an explanation.
: : : Kind Regards,
: : : Jarno de Jonge
------------ End Original Message ------------




 
 Reply 
 
bob sudharmin
Engineering, Reliability and Integrity Eng
Shell Malaysia Trading, Malaysia, Joined Jan 2008, 54

bob sudharmin

Engineering, Reliability and Integrity Eng
Shell Malaysia Trading,
Malaysia,
Joined Jan 2008
54
05:33 Apr-03-2008
Re: comparing UT acceptance ASME VIII, B31.1 and B31.3
My sincere apologies for the inadvertent mistake. I must have overlooked the fact that the statement was meant to be an exclusion of the code's scope. Thank you for the comment.

----------- Start Original Message -----------
: Quote "It is true that B31.3 is less stringent but then again take note it is a piping system designed for and above 0 but less than 105Kpa (15psi)"
: Mr. Sudharmin, this is not correct. 31.3 most certanly allows for pressures above 15psi.
: Regards,
: RB
: :
: : Acceptance criteria does not necessarily be the same when comparison is being made against different code requirements.
: : ASME Viii is a pressure vessel code, B31.1 - Power Piping and B31.3 - Process Piping.
: : It is true that B31.3 is less stringent but then again take note it is a piping system designed for and above 0 but less than 105Kpa (15psi)
: : : Dear Colleagues,
: : : After comparing the acceptance criteria from these 3 codes it seems like the acceptance for B31.3 is much less stringent then for the other two codes.
: : : Is this correct and does anbody know why this is? Or am I just overlooking something in B31.3?
: : : The acceptance for ASME VIII and B31.1 seem to be exactly the same. They don't allow linear discontinuities over 20% DAC and reject rounded discontinuities when they exceed a certain length and 100%DAC.
: : : As far as I can find; B31.3 does not reject rounded discontinuties. And linear discontinuties are allowed to have some length and are allowed to produce indications up to 100% DAC (similar as is allowed for the rounded indications in VIII and B31.1).
: : : Looking forward to an explanation.
: : : Kind Regards,
: : : Jarno de Jonge
------------ End Original Message ------------




 
 Reply 
 

Product Spotlight

TraiNDE UT

TraiNDE UT is a virtual tool associated with a signal database which simulates real inspection con
...
ditions for numerous applications (Type A/V1 block, DAC block, welds and plates).
>

MUSE Mobile Ultrasonic Equipment

The MUSE, a portable ultrasonic imaging system, was developed for in-field inspections of light-weig
...
ht structures. The MUSE consists of a motor-driven manipulator, a water circulation system for the acoustic coupling and a portable ultrasonic flaw detector (USPC 3010). The MUSE provides images of internal defects (A-, B-,C- and D-scan).
>

GUL Subsea Solutions - Screeening & Monitoring

To inspect new and existing subsea lines, you need proven technology and experience. GUL offers it's
...
technology to solve this challenge: GUL Subsea and gMAT Transducer Rings.
>

Robotic laser shearography enables 100% inspection of complex, flight-critical composite structures

An article in “Composites World Magazine” showcases Non Destructive Testing of aero-structures
...
with Laser Shearography. Over the years Dantec Dynamics has supplied many solutions for the aerospace industry. Referring to specific customer projects several of these cases are examined to outline the advantages of using Laser Shearography for automated defect detection.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window