01:06 Apr-07-2008
Ultrasonic test in HDPE

Hi colleagues of NDT, please, i need information, about ultrasonis test in HDPE"s piping, since some years behind use the ASTM F 600 that already is not used: I have my doubts with regard to the use of the UT with the equipments and conventional transducer used for carbon steel.
Thanks


 
 Reply 
 
Rolf Diederichs
Director,
NDT.net, Germany, Joined Nov 1998, 617

Rolf Diederichs

Director,
NDT.net,
Germany,
Joined Nov 1998
617
02:46 Apr-10-2008
Re: Ultrasonic test in HDPE
In NDT.net you find some articles of this topic:

Insight 2007-02
Ultrasonic phased array inspection of electrofusion joints in polyethylene pipes
D. Caravaca, C. Bird, D. Kleiner
TWI Ltd, Cambridge [United Kingdom]
http://www.ndt.net/article/insight/papers/insi.49.2.83.pdf

ECNDT 2006-09
THE ULTRASONIC PHASED ARRAY INSPECTION OF ELECTROFUSION JOINTS IN POLYETHYLENE PIPES
C. Bird, D. Caravaca, D. Kleiner
TWI Ltd, Cambridge [United Kingdom]
http://www.ndt.net/article/ecndt2006/doc/Mo.2.6.2.pdf

NDT.net 1996-04
UT and X-Ray NDT of Butt Fusion Welds in PE Pipe, Overview
G. Georgiou, I. Munns
TWI Ltd, Cambridge [United Kingdom]
http://www.ndt.net/article/twi/twi.htm

----------- Start Original Message -----------
: Hi colleagues of NDT, please, i need information, about ultrasonis test in HDPE"s piping, since some years behind use the ASTM F 600 that already is not used: I have my doubts with regard to the use of the UT with the equipments and conventional transducer used for carbon steel.
: Thanks
------------ End Original Message ------------




 
 Reply 
 
A.Ahmadi
A.Ahmadi
14:52 Jun-22-2011
Re: Ultrasonic test in HDPE
In Reply to Rolf Diederichs at 02:46 Apr-10-2008 .

Dear sir,
my company need buy 1 unit for test hdpe electro fusion fittings 25-160mm

best regards

 
 Reply 
 
coolguy
coolguy
15:29 Jun-22-2011
Re: Ultrasonic test in HDPE
In Reply to A.Ahmadi at 14:52 Jun-22-2011 .

Hello Buddy,

You may contact Olympus NDT as they have already conducted some R7D of these tests.

Please find the link below

http://www.olympus-ims.com/en/applications/ultrasonic-tofd-butt-fusion/

You can contact carl.mercier@olympusndt.com

 
 Reply 
 
Christoph Schnitger
Christoph Schnitger
19:22 Jun-22-2011
Re: Ultrasonic test in HDPE
In Reply to A.Ahmadi at 14:52 Jun-22-2011 .

Dear Sirs,

since 2004 we are offering this kind of UT equipment here on the german market. We used a special kind of phased array system; - it is also a question to have the right probe !

We have this system on stock for different HDPE piping, different wall thicknesses and also
adapters for different fitting styles.

 
 Reply 
 
Raul Leon
Raul Leon
01:59 Nov-02-2011
Re: Ultrasonic test in HDPE
In Reply to vicente domingo encina at 01:06 Apr-07-2008 (Opening).

We have been using TOFD and Phased Array techniques to test joints in HDPE since 2004 in the mining and petrochemical markets. We had, so far, no failures on joints inspected with this methodology and using acceptance and reject criteria developed by large engineering corporations which we have worked in the past. These techniques are getting better with time, and we believe that the codes will include some of these techniques in the future.

 
 Reply 
 
Meh Iskandar
Meh Iskandar
20:50 Nov-06-2011
Re: Ultrasonic test in HDPE
In Reply to vicente domingo encina at 01:06 Apr-07-2008 (Opening).

Hi Encina,

There is a company named "KNDT" that offers some products for your work. It has the worth to see this too.
http://www.kndt.co.kr/us/aim33.htm

It seems that the lack of worldwide accepted code is the main problem in using PA UT in the application of HDPE's inspection.

Good luck

 
 Reply 
 

Product Spotlight

Research Center IDEKO develops an ultrasonic train wheel inspection system for CAF

The Basque Research centre IK4-IDEKO has developed a state-of-the-art ultrasonic inspection system f
...
or the train wheel. This system secures a sound condition of train wheels and is thus a significant contribution to rail transport safety. The device was delivered to CAF recently and its use allows the manufacturer to become an approved supplier of rolling stock in Italy, as it meets the demanding homologation standards of this country. \\\\r\\\\n
>

NEW Wheel Type Phased Array Probe

DOPPLER NEW Wheel Type Phased Array Probe, more stable, new tyre makes lesser acoustic attenuation
...
, much lighter makes easier to handle, more slim size, magnetic and mechanical encoder optional etc...more
>

TESTD-PT SYSTEM

Pulse thermography is a non-contact test method that is ideal for the characterization of thin fil
...
ms and coatings or the detection of defects. With a remarquable short test time and a high detection sensitivity, the Telops TESTD-PT is the perfect tool for non- destructive testing. With such high frame rates, it is even possible to investigate highly conductive or diffusive materials.
>

OPBOX with standard software is able to do all types of inspections and measurements: flaw detection in welds and materials, scanning of objects, testing composite materials, forged and moulded pieces, many UT inspections, measurements of properties of ma

Typical applications: UT measurements with pulse technique, Measurement of thicknesses also at hig
...
h temperatures, Measurements of properties of materials, including fluids and gases We are delivering a standard version of the software (for any Microsoft Windows up to 10 x64 with Microsoft Hardware certification report Approved) and for special needs: SDK with ready to use examples for LabView, MATLAB x64, C++ wrapper for dll, Python and Linux., and also low-level description of how to control our devices directly from any USB tools
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window