AWS D1.1 PT/MT acceptance limit

AWS D1.1 does not specify the acceptance critiera for PT/MT, just one sentence says refer to table 6.1 which is visual inspection acceptance critiera. If a porosity(non piping porosity) was found in Cyclically Loaded Nontubular Connections, How to evaluate it? Can some one explain the PT/MT acceptance critiera?

Thanks!

Eric Chen


 
 Reply 
 
chris s
chris s
07:16 Feb-21-2008
Re: AWS D1.1 PT/MT acceptance limit
----------- Start Original Message -----------
: AWS D1.1 does not specify the acceptance critiera for PT/MT, just one sentence says refer to table 6.1 which is visual inspection acceptance critiera. If a porosity(non piping porosity) was found in Cyclically Loaded Nontubular Connections, How to evaluate it? Can some one explain the PT/MT acceptance critiera?
: Thanks!
: Eric Chen
------------ End Original Message ------------

eric,
what you will need to do is apply the limits in table 6.1 as your acceptance criteria. look in the commentary at c-6.10 note that you do not read bleed out. only the size of the discontinuity.



 
 Reply 
 
DEEPAK SAXENA
DEEPAK SAXENA
09:59 May-31-2008
Re: AWS D1.1 PT/MT acceptance limit
please provide visual acceptance criteria for porosity in TIG welding


 
 Reply 
 
mustafa GONULAL
Engineering,
CIMTAS / ENKA, Turkey, Joined Jun 2008, 8

mustafa GONULAL

Engineering,
CIMTAS / ENKA,
Turkey,
Joined Jun 2008
8
05:26 Jun-04-2008
Re: AWS D1.1 PT/MT acceptance limit
----------- Start Original Message -----------
: please provide visual acceptance criteria for porosity in TIG welding
------------ End Original Message ------------

Aceeptance Limit for PT/MT in AWS is defined as
CJP Groove welds in butt joints transverse to the direction of computes tensile stress shall have no visible piping porosity.
For all other groove welds and fillet welds, the sum of visible piping porosity 1mm or greater in dia. shall not exceed 10mm in any linear inch of weld and shall not exceed 20mm in any 12in. length of weld.


 
 Reply 
 
mike
mike
01:32 Aug-23-2014
Re: AWS D1.1 PT/MT acceptance limit
In Reply to chris s at 07:16 Feb-21-2008 .

AWS c-6.10 only refers to clause 6.14.4 for MT test which is very general. It basically ask for app the acceptance criteria that are in Section 6, part C, whichever is applicable. Can any one elaborate what "whichever applicable" mean? In section 6, partc there are requirements for UT and RT. Should one is applicable, ut or rt?

thanks,

 
 Reply 
 
mike
mike
01:47 Aug-23-2014
Re: AWS D1.1 PT/MT acceptance limit
In Reply to mike at 01:32 Aug-23-2014 .

AWS c-6.10 only refers to clause 6.14.4 for MT test which is very general. It basically says " acceptance shall be in conformance with Section6, part C, of this code, whichever is applicable". Can any one elaborate what "whichever applicable" mean? In section 6, part C there are only requirements for UT and RT tests. which one is applicable, UT or RT?
I assume RT, any comment?

thanks,

 
 Reply 
 

Product Spotlight

TraiNDE UT

TraiNDE UT is a virtual tool associated with a signal database which simulates real inspection con
...
ditions for numerous applications (Type A/V1 block, DAC block, welds and plates).
>

Echomac® Small

Available with up to eight channels of electronics to detect and evaluate thickness, flaws and eccen
...
tricity, this UT tester is housed in a convenient, smaller cabinet. This instrument can be used in conjunction with bubbler or immersion tank systems, or with a test bench or in laboratory applications. The Echomac® Small is available in the FD4, FD6 or FD6A versions.
>

Content on Demand by Eddyfi Technologies

Finding yourself in front of a screen practicing safe social distancing instead of out in the fiel
...
d? At Eddyfi Technologies, we are doing our part in helping you be better prepared for what comes next. We introduce to you Eddyfi on Demand. Fill your schedule with webinars, how-to videos, informative technical papers and our NEW addition: Eddyfi Academy. There, you will have access to FREE online courses and obtain certificates of attendance once completed in order for you to include these e-learning sessions in your log of required training hours. Join us today. Stay safe, stay Beyond Current.
>

NDT.net launches mobile-friendly design

NDT.net has revamped its website providing a mobile-friendly design.The front page received a comp
...
letely new design and all other sections are now reacting responsively on mobile devices. This has been a major step to make our website more user- friendly.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window