ras
ras
06:56 Aug-12-2008
oxie layer measurment in boiler tube

pls inform proceduer to measure thickness of oxide layer through A-Scan instrument thickness gauge step by step for above measurment please also inform what display and where cursor to be set/gate


 
 Reply 
 
Tom Nelligan
Engineering,
retired, USA, Joined Nov 1998, 390

Tom Nelligan

Engineering,
retired,
USA,
Joined Nov 1998
390
09:11 Aug-12-2008
Re: oxie layer measurment in boiler tube
The specific answer to your question depends on which gage and transducer you are using. Please provide that additional information. If you're using Panametrics-NDT products I can help with the setup, and if you're using something from one of our competitors perhaps someone from that company can step in.

In general, you will always measure from the echo representing the steel/oxide boundary to the echo representing the inside of the oxide layer, so gates are set for detection of those echoes. Some typical waveforms can be found in the application note at the link below.


----------- Start Original Message -----------
: pls inform proceduer to measure thickness of oxide layer through A-Scan instrument thickness gauge step by step for above measurment please also inform what display and where cursor to be set/gate
------------ End Original Message ------------




 
 Reply 
 
RickyOng88
Director, -
ASNT, Singapore, Joined Aug 2008, 12

RickyOng88

Director, -
ASNT,
Singapore,
Joined Aug 2008
12
05:34 Aug-14-2008
Re: oxie layer measurment in boiler tube
----------- Start Original Message -----------
: pls inform proceduer to measure thickness of oxide layer through A-Scan instrument thickness gauge step by step for above measurment please also inform what display and where cursor to be set/gate
------------ End Original Message ------------
Whether the Boiler is Fired Tube or Water Tube the best method to be used for measuring the whole length of tube (except bends) is by Internal Rotary Inspection System (IRIS). Spot ultrasonic thickness measurement not good method for boiler tubes only area you could access.



 
 Reply 
 
David Hermanutz
Consultant,
Hbndt.com, China, Joined Jul 2012, 85

David Hermanutz

Consultant,
Hbndt.com,
China,
Joined Jul 2012
85
02:50 Aug-21-2008
Re: oxie layer measurment in boiler tube
----------- Start Original Message -----------
: : pls inform proceduer to measure thickness of oxide layer through A-Scan instrument thickness gauge step by step for above measurment please also inform what display and where cursor to be set/gate
: Whether the Boiler is Fired Tube or Water Tube the best method to be used for measuring the whole length of tube (except bends) is by Internal Rotary Inspection System (IRIS). Spot ultrasonic thickness measurement not good method for boiler tubes only area you could access.
------------ End Original Message ------------

The Olympus NDT / Panametrics 37DL Plus has a feature that handles this, please contact your local sales rep and they can show you the way out of your dilemma.

Regards,

David Hermanutz
www.HBNDT.com




 
 Reply 
 
RickyOng88
Director, -
ASNT, Singapore, Joined Aug 2008, 12

RickyOng88

Director, -
ASNT,
Singapore,
Joined Aug 2008
12
07:11 Aug-22-2008
Re: oxie layer measurment in boiler tube
----------- Start Original Message -----------
: : pls inform proceduer to measure thickness of oxide layer through A-Scan instrument thickness gauge step by step for above measurment please also inform what display and where cursor to be set/gate

: If you only want to measure thickness of oxide layer try using coating thickness gauge, we use it on stainless steel cladded to steel plate for production oil tanker. We tried using "A" Scan but failed.
------------ End Original Message ------------

Whether the Boiler is Fired Tube or Water Tube the best method to be used for measuring the whole length of tube (except bends) is by Internal Rotary Inspection System (IRIS) an ultrasonic method, as well.

Maybe I misunderstood you for wanted to measure boiler tube thickness.


 
 Reply 
 

Product Spotlight

VOGT Ultrasonics awarded innovation champion

Let go of the old and try something new. VOGT convinced the jury in the 27th round of the TOP 100
...
innovation competition. Our team is very pleased to officially belong to the TOP 100 in Germany!
>

Research Center IDEKO develops an ultrasonic train wheel inspection system for CAF

The Basque Research centre IK4-IDEKO has developed a state-of-the-art ultrasonic inspection system f
...
or the train wheel. This system secures a sound condition of train wheels and is thus a significant contribution to rail transport safety. The device was delivered to CAF recently and its use allows the manufacturer to become an approved supplier of rolling stock in Italy, as it meets the demanding homologation standards of this country. \\\\r\\\\n
>

FD800 Bench Top Flaw Detectors

The bench-top FD800 flaw detector range combines state-of-the-art flaw detection with advanced mater
...
ial thickness capabilities. Designed for use in the laboratory these gauges are the tool you need for all your flaw detecting needs.
>

SITEX CPSERIES

Teledyne ICM’s CPSERIES has been designed with a view to revolutionizing the handling and perfor
...
mances of portable X-Ray sets. Despite having managed to halve the weight of similar portable X-Ray generators available on the market (while continuing to provide the same power output), the SITEX CPSERIES generators feature a shutter, a laser pointer, a beryllium window, an aluminum filter and two integrated diaphragms (customized sizes are available upon request). Without compromising the robustness and reliability for which ICM products are renowned, the small size and light weight of the SITEX CPSERIES will radically change the way that you perform your RT inspections. And you will see a positive impact in terms of both quality and return on investment (ROI).
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window