oxie layer measurment in boiler tube

pls inform proceduer to measure thickness of oxide layer through A-Scan instrument thickness gauge step by step for above measurment please also inform what display and where cursor to be set/gate


 
 Reply 
 
Tom Nelligan
Engineering,
retired, USA, Joined Nov 1998, 390

Tom Nelligan

Engineering,
retired,
USA,
Joined Nov 1998
390
09:11 Aug-12-2008
Re: oxie layer measurment in boiler tube
The specific answer to your question depends on which gage and transducer you are using. Please provide that additional information. If you're using Panametrics-NDT products I can help with the setup, and if you're using something from one of our competitors perhaps someone from that company can step in.

In general, you will always measure from the echo representing the steel/oxide boundary to the echo representing the inside of the oxide layer, so gates are set for detection of those echoes. Some typical waveforms can be found in the application note at the link below.


----------- Start Original Message -----------
: pls inform proceduer to measure thickness of oxide layer through A-Scan instrument thickness gauge step by step for above measurment please also inform what display and where cursor to be set/gate
------------ End Original Message ------------




 
 Reply 
 
RickyOng88
Director, -
ASNT, Singapore, Joined Aug 2008, 12

RickyOng88

Director, -
ASNT,
Singapore,
Joined Aug 2008
12
05:34 Aug-14-2008
Re: oxie layer measurment in boiler tube
----------- Start Original Message -----------
: pls inform proceduer to measure thickness of oxide layer through A-Scan instrument thickness gauge step by step for above measurment please also inform what display and where cursor to be set/gate
------------ End Original Message ------------
Whether the Boiler is Fired Tube or Water Tube the best method to be used for measuring the whole length of tube (except bends) is by Internal Rotary Inspection System (IRIS). Spot ultrasonic thickness measurement not good method for boiler tubes only area you could access.



 
 Reply 
 
David Hermanutz
Consultant,
Hbndt.com, China, Joined Jul 2012, 85

David Hermanutz

Consultant,
Hbndt.com,
China,
Joined Jul 2012
85
02:50 Aug-21-2008
Re: oxie layer measurment in boiler tube
----------- Start Original Message -----------
: : pls inform proceduer to measure thickness of oxide layer through A-Scan instrument thickness gauge step by step for above measurment please also inform what display and where cursor to be set/gate
: Whether the Boiler is Fired Tube or Water Tube the best method to be used for measuring the whole length of tube (except bends) is by Internal Rotary Inspection System (IRIS). Spot ultrasonic thickness measurement not good method for boiler tubes only area you could access.
------------ End Original Message ------------

The Olympus NDT / Panametrics 37DL Plus has a feature that handles this, please contact your local sales rep and they can show you the way out of your dilemma.

Regards,

David Hermanutz
www.HBNDT.com




 
 Reply 
 
RickyOng88
Director, -
ASNT, Singapore, Joined Aug 2008, 12

RickyOng88

Director, -
ASNT,
Singapore,
Joined Aug 2008
12
07:11 Aug-22-2008
Re: oxie layer measurment in boiler tube
----------- Start Original Message -----------
: : pls inform proceduer to measure thickness of oxide layer through A-Scan instrument thickness gauge step by step for above measurment please also inform what display and where cursor to be set/gate

: If you only want to measure thickness of oxide layer try using coating thickness gauge, we use it on stainless steel cladded to steel plate for production oil tanker. We tried using "A" Scan but failed.
------------ End Original Message ------------

Whether the Boiler is Fired Tube or Water Tube the best method to be used for measuring the whole length of tube (except bends) is by Internal Rotary Inspection System (IRIS) an ultrasonic method, as well.

Maybe I misunderstood you for wanted to measure boiler tube thickness.


 
 Reply 
 

Product Spotlight

A1525 SOLO

A1525 Solo – the most compact and affordable TMF unit with two phased array transducers and 3D v
...
isualization and analysis software in standard delivery set. A compact, ergonomic and easy to handheld Phased Array unit based on Total Focusing Method for easy-going imaging of inspection objects with two-dimensional and three-dimensional visualization and evaluation of inspection results.
>

32:128PR PAUT & 2-ch TOFD Flaw Detector: SyncScan 2

●32:128PR PAUT with optional 2-ch TOFD to maximize your efficiency ●Support PR mode for corrosi
...
on inspection ●Multiple solutions for welds & corrosion ●Faster scan speed (Approximately 3 meters/minute) ●Light weight: 4kg only including battery
>

Varex Imaging Large Field of View (FOV) Digital Detector Arrays (DDAs)

A larger FOV DDA can reduce the space and volume of the X-ray inspection system on the factory floor
...
, enable faster scanning times, better throughput and better resolution images at a lower dose. Customers can also save time and money. With these benefits in mind, Varex Imaging has designed a family of large FOV detectors (4343HE, XRD 1611, 4343DX-I, 4343CT) for our industrial imaging customers.
>

HD-CR 35 NDT Computed Radiography System

Portable high-resolution CR scanner for all radiography applications - weld testing, profile images
...
and aerospace. No matter what type of radiographic testing you are performing, the unique TreFoc Technology of the HD-CR 35 NDT imaging plate scanner always guarantees the highest image quality.
>