Maximum penetration of Ir-192 in steel

Hi,
We are using Ir-192 to examine the casting quality of a steel part with maximum thickness 95.25mm:
(1) Is Ir-192 OK for this application?
(2) Does the decay influence the maximum penetration thickness?
Many thanks,
Pengzhu



 
 Reply 
 
tj
tj
07:11 Nov-14-2008
Re: Maximum penetration of Ir-192 in steel
----------- Start Original Message -----------
: Hi,
: We are using Ir-192 to examine the casting quality of a steel part with maximum thickness 95.25mm:
: (1) Is Ir-192 OK for this application?
: (2) Does the decay influence the maximum penetration thickness?
: Many thanks,
: Pengzhu
------------ End Original Message ------------

This would be working at the upper practical limit of Ir192. The energy levels would remain the same with decay. However, with loss of activity comes increased shot time and at 3in. of steel it would be impractical for normal use. Better to use higher energy x-ray or cobalt60 gamma.


 
 Reply 
 
Juan Amado
Engineering, Inspection
Arco Industrial, S.A., Panama, Joined Nov 2001, 44

Juan Amado

Engineering, Inspection
Arco Industrial, S.A.,
Panama,
Joined Nov 2001
44
09:53 Nov-14-2008
Re: Maximum penetration of Ir-192 in steel
----------- Start Original Message -----------
: : Hi,
: : We are using Ir-192 to examine the casting quality of a steel part with maximum thickness 95.25mm:
: : (1) Is Ir-192 OK for this application?
: : (2) Does the decay influence the maximum penetration thickness?
: : Many thanks,
: : Pengzhu
: This would be working at the upper practical limit of Ir192. The energy levels would remain the same with decay. However, with loss of activity comes increased shot time and at 3in. of steel it would be impractical for normal use. Better to use higher energy x-ray or cobalt60 gamma.
------------ End Original Message ------------


If 95mm is the maximum thickness, but you have thinner sections, you could probably gain valuable information about the part using Ir192, however, if you are looking to get a good density reading at the thickest portion of the casting you probably will not get it with this source.
Hope this helps, regards,
Juan Amado



 
 Reply 
 
Peter Alfers
Peter Alfers
09:53 Nov-16-2008
Re: Maximum penetration of Ir-192 in steel
you can use Ir 192 in conjunction with two Films how will
exposure at once. Than you need the half time for your right density .For the interpretation use the films lying upon each other.


 
 Reply 
 

Product Spotlight

Compact NDT inspection-heads for measurements with active thermography

The compact inspection head is suitable for thermographic ndt tasks. The uncooled infrared camera
...
is specially developed for NDI-tasks and offers a thermal sensitivity until now known only from thermal imagers with cooled detector. All required components and functions are integrated into the inspection-head. You will only need an ethernet cable to connect the sensor with the evaluation system.
>

Portable Ground Penetrating Radar - Proceq GP8000

The Proceq GP8000 portable ground penetrating radar instrument is the beginning of a new era in ND
...
T. The outstanding, patented ultra- wideband technology combined with a compact wireless probe delivers unmatched industry performance. Proceq GP8000 is the world’s first large-scale inspection solution that utilizes Augmented Reality in industrial applications.
>

Research and Application Development For NDT

Acuren’s Research and Application Development specializes in the development of advanced ultraso
...
nic inspection techniques and systems for challenging inspection applications, with an emphasis on practical solutions which are field deployable. Services include manual and automated ultrasonic inspection system development, inspection technique optimization using laboratory scale studies and ultrasonic modeling (CIVA, BeamTool), preparing technical justification for technique evaluation and qualification (Probability of Detection and sizing accuracy studies), inspection/calibration/analysis procedure preparation to support field deployment of custom techniques, and development of custom imaging algorithms to support challenging inspection applications.
>

NDT Master Lecturer

In the program both university professors and practitioners will give lectures, which guarantees the
...
oretical depth and practical inside. Academic Director: Prof. Dr. Christian Boller
The following lecturers are not complete: Prof. Tadeusz Stepinski, Prof. Wieslaw Staszewski, Prof. Frank Walther, Prof. Giovanni Bruno, Prof. Gerd Dobmann, Prof. Philippe Guy
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window