balwinder singh
balwinder singh
09:55 Nov-30-2008
Selection of IQI/Radition source

dear experts,

we are doing radiographic testing of piping weldments,the dimension of our job as detail given below:-

OD OF PIPE/Single wall thickness

141/6.55 mm
168.3/7.11 mm

class of testing EN 1435 CLASS B

question is:-
what type of source we have to used.

which wire should be vissible on radiograph.(IQI 10 10 FE EN).

also let me know what is penetrated thickness.
thanks



    
 
 Reply 
 
Nigel Armstrong
Engineering, - Specialist services
United Kingdom, Joined Oct 2000, 1096

Nigel Armstrong

Engineering, - Specialist services
United Kingdom,
Joined Oct 2000
1096
01:56 Dec-01-2008
Re: Selection of IQI/Radition source
Balwinder

Contract documentation should specify if there are any limitations further than the moninated Code. So the Owner's specification may say "X-ray only", even though the Codes usually permit either X or gamma within material thickness limitations. Low kV X-ray gives better images in most cases than commercially available gamma sources, though I have read that Selenium can give good results on thinner materials.

Your required visible wire is one that indicates better then 2% sensitivity so its diameter should be less than 6.55mm x 0.02 = 0.131mm or 7.11mm x 0.02 = 0.142mm

Penetrated thickness for Ug unsharpness calculation is the single wall thickness (6.55 or 7.11mm) + single measured weld reinforcement.

Hope this helps

Nigel

----------- Start Original Message -----------
: dear experts,
: we are doing radiographic testing of piping weldments,the dimension of our job as detail given below:-
: OD OF PIPE/Single wall thickness
: 141/6.55 mm
: 168.3/7.11 mm
: class of testing EN 1435 CLASS B
: question is:-
: what type of source we have to used.
: which wire should be vissible on radiograph.(IQI 10 10 FE EN).
: also let me know what is penetrated thickness.
: thanks
------------ End Original Message ------------




    
 
 Reply 
 
annonym
annonym
07:59 Dec-01-2008
Re: Selection of IQI/Radition source
Selen 75, Wire 13 or 14 should be visible.

----------- Start Original Message -----------
: Balwinder
: Contract documentation should specify if there are any limitations further than the moninated Code. So the Owner's specification may say "X-ray only", even though the Codes usually permit either X or gamma within material thickness limitations. Low kV X-ray gives better images in most cases than commercially available gamma sources, though I have read that Selenium can give good results on thinner materials.
: Your required visible wire is one that indicates better then 2% sensitivity so its diameter should be less than 6.55mm x 0.02 = 0.131mm or 7.11mm x 0.02 = 0.142mm
: Penetrated thickness for Ug unsharpness calculation is the single wall thickness (6.55 or 7.11mm) + single measured weld reinforcement.
: Hope this helps
: Nigel
: : dear experts,
: : we are doing radiographic testing of piping weldments,the dimension of our job as detail given below:-
: : OD OF PIPE/Singlewall thickness
: : 141/6.55 mm
: : 168.3/7.11 mm
: : class of testing EN 1435 CLASS B
: : question is:-
: : what type of source we have to used.
: : which wire should be vissible on radiograph.(IQI 10 10 FE EN).
: : also let me know what is penetrated thickness.
: : thanks
------------ End Original Message ------------




    
 
 Reply 
 

Product Spotlight

Combination of Digital Image Correlation and Thermographic Measurements

The combination of measuring results from the digital image correlation (ARAMIS, DIC) and temperat
...
ure measuring data from infrared cameras permits the simultaneous analysis of the thermal and mechanical behavior of test specimens in the materials and components testing field.
>

IntraPhase Athena Phased Array System

The Athena Phased Array system, manufactured by WesDyne NDE Products & Technology, consists of a pha
...
sed array acquisition system and PC running IntraSpect software. A PC is used to perform acquisition, analysis and storage of the data. System hardware is capable of operating up to four data sets with any combination of phased array or conventional UT probes. NOW AVAILABLE IN 64-64 CONFIGURATION.
>

High-end Ultrasonic Flaw Detector with 32:128PR PAUT and 2-ch TOFD: SyncScan 2

SIUI’s newly launched SyncScan 2, is a high-end ultrasonic flaw detector with 32:128PR PAUT and
...
2-ch TOFD, which can maximize your efficiency for PA and TOFD. ● Support PA/TOFD/UT ● 32-ch PA is more suitable for inspection on extra-thick wall and high-attenuation material. ● 32-ch PA and 2-ch TOFD work simultaneously. ● Support PR mode for corrosion inspection.
>

Magnetic X-Ray Pipeline Crawler

Zhong Yi brand pipeline crawler is magnetic/micro-video controlled crawler with DC X ray unit inst
...
alled for checking welding of pipeline. Move steadily inside the pipeline 6''-60''diameter with speed of up to 18m/min, Max. moving diatance 5 kilometers and provide the efficient inspection of the pipeline.
>