Selection of IQI/Radition source

dear experts,

we are doing radiographic testing of piping weldments,the dimension of our job as detail given below:-

OD OF PIPE/Single wall thickness

141/6.55 mm
168.3/7.11 mm

class of testing EN 1435 CLASS B

question is:-
what type of source we have to used.

which wire should be vissible on radiograph.(IQI 10 10 FE EN).

also let me know what is penetrated thickness.
thanks



    
 
 Reply 
 
Nigel Armstrong
Engineering, - Specialist services
United Kingdom, Joined Oct 2000, 1096

Nigel Armstrong

Engineering, - Specialist services
United Kingdom,
Joined Oct 2000
1096
01:56 Dec-01-2008
Re: Selection of IQI/Radition source
Balwinder

Contract documentation should specify if there are any limitations further than the moninated Code. So the Owner's specification may say "X-ray only", even though the Codes usually permit either X or gamma within material thickness limitations. Low kV X-ray gives better images in most cases than commercially available gamma sources, though I have read that Selenium can give good results on thinner materials.

Your required visible wire is one that indicates better then 2% sensitivity so its diameter should be less than 6.55mm x 0.02 = 0.131mm or 7.11mm x 0.02 = 0.142mm

Penetrated thickness for Ug unsharpness calculation is the single wall thickness (6.55 or 7.11mm) + single measured weld reinforcement.

Hope this helps

Nigel

----------- Start Original Message -----------
: dear experts,
: we are doing radiographic testing of piping weldments,the dimension of our job as detail given below:-
: OD OF PIPE/Single wall thickness
: 141/6.55 mm
: 168.3/7.11 mm
: class of testing EN 1435 CLASS B
: question is:-
: what type of source we have to used.
: which wire should be vissible on radiograph.(IQI 10 10 FE EN).
: also let me know what is penetrated thickness.
: thanks
------------ End Original Message ------------




    
 
 Reply 
 
annonym
annonym
07:59 Dec-01-2008
Re: Selection of IQI/Radition source
Selen 75, Wire 13 or 14 should be visible.

----------- Start Original Message -----------
: Balwinder
: Contract documentation should specify if there are any limitations further than the moninated Code. So the Owner's specification may say "X-ray only", even though the Codes usually permit either X or gamma within material thickness limitations. Low kV X-ray gives better images in most cases than commercially available gamma sources, though I have read that Selenium can give good results on thinner materials.
: Your required visible wire is one that indicates better then 2% sensitivity so its diameter should be less than 6.55mm x 0.02 = 0.131mm or 7.11mm x 0.02 = 0.142mm
: Penetrated thickness for Ug unsharpness calculation is the single wall thickness (6.55 or 7.11mm) + single measured weld reinforcement.
: Hope this helps
: Nigel
: : dear experts,
: : we are doing radiographic testing of piping weldments,the dimension of our job as detail given below:-
: : OD OF PIPE/Singlewall thickness
: : 141/6.55 mm
: : 168.3/7.11 mm
: : class of testing EN 1435 CLASS B
: : question is:-
: : what type of source we have to used.
: : which wire should be vissible on radiograph.(IQI 10 10 FE EN).
: : also let me know what is penetrated thickness.
: : thanks
------------ End Original Message ------------




    
 
 Reply 
 

Product Spotlight

Cygnus 6+ PRO Multi-Mode Ultrasonic Thickness Gauge

The Cygnus 6+ PRO thickness gauge is the most advance gauge within the Cygnus range with key featu
...
res including: comprehensive data logging; A-scan and B-scan display; manual gain control; Bluetooth connectivity; and much more. With its unique dual display and three measuring modes (Multiple-Echo, Echo-Echo and Single-Echo), this surface thickness gauge offers maximum versatility for inspections.
>

TOPAZ® 64: Fully Integrated Portable 32 or 64 Channel PAUT Instrument with FMC & TFM

Introducing TOPAZ64, the industry’s most intelligent fully integrated, portable 32 or 64-channel
...
phased array ultrasound (UT) instrument. TOPAZ64 combines code-compliant phased array UT with the industry’s most advanced full matrix capture (FMC) and total focusing method (TFM) capabilities. Featuring the highest acquisition frequency in its class, high resolution FMC and a 12” multi-touchscreen, users can easily visualize even the smallest flaws. TOPAZ64 can generate a bipolar pulse that provides more acoustic energy versus previous models for punching through thick components. The result is a portable tool that delivers increased inspection coverage, more accurate signals, and the ability to handle all UT inspections in one package. TOPAZ64 is ideal for challenging applications in transportation, oil and gas, manufacturing and power generation.
>

Semi-Automated Phased Array Immersion System for Small Composite Parts

Turn-key semi-automated system as an improved and affordable solution for inspection of small comp
...
osite parts. Includes support table, immersion tank, scanner, PA instrument, PC, Analysis software, database, wedge management and other options.
>

NDT.net launches mobile-friendly design

NDT.net has revamped its website providing a mobile-friendly design.The front page received a comp
...
letely new design and all other sections are now reacting responsively on mobile devices. This has been a major step to make our website more user- friendly.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window