Thin Gauge Steel Tubes

I am looking for a reliable way to UT thin gauge, under 5/16", steel tube that has a circumferential joint joined utilizing a backing bar.


 
 Reply 
 
Tom Nelligan
Engineering,
retired, USA, Joined Nov 1998, 390

Tom Nelligan

Engineering,
retired,
USA,
Joined Nov 1998
390
09:30 Jun-23-2000
Re: Thin Gauge Steel Tubes
: I am looking for a reliable way to UT thin gauge, under 5/16", steel tube that has a circumferential joint joined utilizing a backing bar.

I'm not sure I'm properly visualizing what you're doing, but if it's a brazed or welded joint, we may be able to do something with small diameter, sharply focussed immersion transducers and appropriate fixturing. The tube diameter itself is not a problem. If it's just mechanically clamped, on the other hand, it's not a good application for ultrasonic flaw detection.

I'd be happy to look at a drawing if you can send one.

--Tom Nelligan
Panametrics, Inc.




 
 Reply 
 
Joseph Pascente
Engineering
Lixi, Inc., USA, Joined Nov 1998, 39

Joseph Pascente

Engineering
Lixi, Inc.,
USA,
Joined Nov 1998
39
07:02 Jun-25-2000
Re: Thin Gauge Steel Tubes
Dear Tom,

Go to www.lixi.com and then to Profiler. This non
contact wall thickness gauge will measure the wall
thickness of thin gauge steel tubes.


Regards,

Lixi, Inc.


Joe Pascente


 
 Reply 
 
Rick Pfannenstiel
Consultant
Spin LLC, USA, Joined Jun 2000, 1

Rick Pfannenstiel

Consultant
Spin LLC,
USA,
Joined Jun 2000
1
04:14 Jun-29-2000
Re: Thin Gauge Steel Tubes
We have been inspecting buttwelds in .056"T by 1.0" diameter buttwelds in inconnel tubing with great success using FAST ultrasonics. The backing ring should not be a problem. Not sure that this application is close to what you are doing. If you would like more information please email me.


 
 Reply 
 
Alexander Tsankov
Alexander Tsankov
01:17 Aug-03-2000
Carbon Steel Tubes
Dear Sirs,
I am interested in Carbon Steel Tubes with diameter 40-48mm. If you can help me please send me Reply on my e-mail: powercom@netbg.com.

Sincerelly Yours
A. Tsankov


 
 Reply 
 

Product Spotlight

Echomac® PA Tube Weld Tester

The new robotic Echomac® PA TW is an operator friendly test system for detecting weld zone defects
...
in tube and pipe caused by scarfing or welding processes. Electronic scanning ensures that the entire weld zone is covered without the need for mechanical movement or operator adjustment.
>

Scatter Correction for Industrial Cone-Beam Computed Tomography (CBCT)

Download our white paper on Scatter Correction for Industrial Cone-Beam Computed Tomography (CBCT)
...
Using 3D VSHARP, a fast GPU-Based Linear Boltzmann Transport Equation Solver here: http://bit.ly/2Y0t78P
>

Ultrasonic Squirter/Gantry System

TecScan’s NDT Ultrasonic Gantry Systems are industrial Squirter scanners designed for non-destru
...
ctive quality testing and raster scanning of large structures and parts. The Gantry Systems are usually composed of an Industrial Mechanical Scanner and a Control Room with System Workstation.
>

VOGT Ultrasonics awarded innovation champion

Let go of the old and try something new. VOGT convinced the jury in the 27th round of the TOP 100
...
innovation competition. Our team is very pleased to officially belong to the TOP 100 in Germany!
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window