NDT Folks,
In reviewing ASTM E1444 (1999), I became hung up on a requirement described in section 5.5 "Examination Sequence". It is recommended that "parts heat treated to an ultimate tensile strength of 180 ksi or higher that are heat treated and subsequently electroplated shall be inspected after the electroplating operation".
My questions are: does this suggest that parts having an ultimate tensile strength of 180 ksi or higher should be inspected twice, once prior to electroplating and once after electroplating? Would one inspection after electroplating be sufficient (plating thickness of less than .001")? What are the types of discontinuities to be concerned with? If the plating process is tightly controled, do you still need the post plating inspection?

Just curious if anyone has had any personal experience in dealing with this requirement, and if so how it was handled.

Thank you,
Brian


 
 Reply 
 
Ed Ginzel
R & D, -
Materials Research Institute, Canada, Joined Nov 1998, 1304

Ed Ginzel

R & D, -
Materials Research Institute,
Canada,
Joined Nov 1998
1304
07:36 Jul-13-2000
Re: ASTM E1444 Requirement
Brian:
ASTM 1444 Para. 5.5 is fairly specific about this.
It requires that WHEN specified, MPI is done after operations that could cause surface or near surface defects.
Then it goes on to state that MPI is to be done prior to coating unless otherwise approved by the contracting agency or as approved by para. 6.1.3. (6.1.3 describes conditions that would limit MPI through coatings).
Not withstanding 6.1.3, 5.5 goes on to state that MPI will ALSO be done on parts heat treated to 180ksi or higher and subsequently electroplated, AFTER electroplating.
This would therefore imply MPI is needed before and after electroplating unless the contracting agency does not require the MPI prior to electroplating (the requirement for MPI after electroplating is a SHALL condition so MUST be done).

Ed

: NDT Folks,
: In reviewing ASTM E1444 (1999), I became hung up on a requirement described in section 5.5 "Examination Sequence". It is recommended that "parts heat treated to an ultimate tensile strength of 180 ksi or higher that are heat treated and subsequently electroplated shall be inspected after the electroplating operation".
: My questions are: does this suggest that parts having an ultimate tensile strength of 180 ksi or higher should be inspected twice, once prior to electroplating and once after electroplating? Would one inspection after electroplating be sufficient (plating thickness of less than .001")? What are the types of discontinuities to be concerned with? If the plating process is tightly controled, do you still need the post plating inspection?

: Just curious if anyone has had any personal experience in dealing with this requirement, and if so how it was handled.

: Thank you,
: Brian




 
 Reply 
 
Brian M. Younce
Brian M. Younce
02:20 Jul-13-2000
Re: ASTM E1444 Requirement
>Thank you for your response. Is it safe to say the reason for the inspection after electroplating is based on a concern of hydrogen embrittlement cracking? If so, what is the nature of hydrogen embrittlement cracking??? Is it always an obvious condition (gross indications) or is it more of a material related condition which often goes undetected but serves as a vehicle for a stress/fatigue related crack in years to come???
>
>Regards,
>Brian

: Brian:
: ASTM 1444 Para. 5.5 is fairly specific about this.
: It requires that WHEN specified, MPI is done after operations that could cause surface or near surface defects.
: Then it goes on to state that MPI is to be done prior to coating unless otherwise approved by the contracting agency or as approved by para. 6.1.3. (6.1.3 describes conditions that would limit MPI through coatings).
: Not withstanding 6.1.3, 5.5 goes on to state that MPI will ALSO be done on parts heat treated to 180ksi or higher and subsequently electroplated, AFTER electroplating.
: This would therefore imply MPI is needed before and after electroplating unless the contracting agency does not require the MPI prior to electroplating (the requirement for MPI after electroplating is a SHALL condition so MUST be done).

: Ed

: : NDT Folks,
: : In reviewing ASTM E1444 (1999), I became hung up on a requirement described in section 5.5 "Examination Sequence". It is recommended that "parts heat treated to an ultimate tensile strength of 180 ksi or higher that are heat treated and subsequently electroplated shall be inspected after the electroplating operation".
: : My questions are: does this suggest that parts having an ultimate tensile strength of 180 ksi or higher should be inspected twice, once prior to electroplating and once after electroplating? Would one inspection after electroplating be sufficient (plating thickness of less than .001")? What are the types of discontinuities to be concerned with? If the plating process is tightly controled, do you still need the post plating inspection?

: : Just curious if anyone has had any personal experience in dealing with this requirement, and if so how it was handled.

: : Thank you,
: : Brian




 
 Reply 
 

Product Spotlight

ISONIC 3510

Very Powerful Superior Performance Extremely Portable Smart Phased Array Ultrasonic Flaw Detector an
...
d Recorder with 2 Conventional UT and TOFD Channels uniquely combines PA, single- and multi-channel conventional UT, and TOFD modalities providing 100% raw data recording and imaging. Suitable for all kinds of every-day ultrasonic inspections
>

Ultrasonic Squirter/Gantry System

TecScan’s NDT Ultrasonic Gantry Systems are industrial Squirter scanners designed for non-destru
...
ctive quality testing and raster scanning of large structures and parts. The Gantry Systems are usually composed of an Industrial Mechanical Scanner and a Control Room with System Workstation.
>

VOGT Ultrasonics awarded innovation champion

Let go of the old and try something new. VOGT convinced the jury in the 27th round of the TOP 100
...
innovation competition. Our team is very pleased to officially belong to the TOP 100 in Germany!
>

FMC/TFM

Next generation for Phased Array UT is here now with FMC/TFM! Have higher resolution imaging, impr
...
oved signal to noise ratio, characterize, size and analyze defects better with access to several wave mode views and save raw FMC data for higher quality analysis.  Some of the benefits are:
  • Beautiful Image! Easier to understand what you're looking at
  • Completely focused in entire image or volume
  • Much easier to define setups before inspection
  • Easier to decipher geometry echoes from real defects
  • Oriented defects (e.g. cracks) are imaged better
  • See image from different wave modes from one FMC inspection
  • FMC data can be reprocessed/analyzed without going back to the field
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window