Technical Discussions
Jedispin
Jedispin
06:59 Aug-18-2009
Subsurface crack detection by MT in Martensitic Stainsless Steel

Hi,

I would like to have some information regarding subsurface crack detection by MT in Martensitic Stainsless Steel. I would like to know, what is the maximum depth that we can detect such a crack for martensitic stainless steel.

Do a study has been already done regarding subsurface crack detection on different material.

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 869

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
869
03:57 Aug-19-2009
Re: Subsurface crack detection by MT in Martensitic Stainsless Steel
In Reply to Jedispin at 06:59 Aug-18-2009 (Opening).

Hi,

I will answer your question assuming that you are inspecting parts of that material on a regular basis. Maybe you should get a Ketos Ring of a similar material. This way, you will be able to properly verify the sensitivity of your system and will know exactly how deep you can go. The drawing can be found in ASTM E1444.

 
 Reply 
 
John Brunk
Engineering, NDT Level III
Self employed, part-time, USA, Joined Oct 1999, 161

John Brunk

Engineering, NDT Level III
Self employed, part-time,
USA,
Joined Oct 1999
161
06:46 Aug-19-2009
Re: Subsurface crack detection by MT in Martensitic Stainsless Steel
In Reply to Jedispin at 06:59 Aug-18-2009 (Opening).

Martensitic stainless steels, including maraging steel that has not been heat
treated to reform a substantial percentage of austenite, has extremely
limited depth of penetration for very low-frequency eddy current inspection.
Based on this I would be surprised if you could detect subsurface defects with
an electromagnetic yoke. With full-wave rectified current and high amperage
and a Ketos-type ring as Michel suggested, you might find an answer that
pleases you. There are both ferromagnetic and non-ferromagnetic forms of
martensite, but the ferromagnetic form structure often predominates, especially
in maraging steels.

 
 Reply 
 

Product Spotlight

Eddy Current inspection : RotoETscan Rotating Head

The rotating head RotoETscan detects the presence of longitudinal surface or sub surface defects a
...
t high speed. The rotating head is often installed directly on the production line. It is generally dedicated to the control of long products such as tubes, bars and wires, made of ferrous or non-ferrous material. It can also be used for inspection of small parts (billets).
>

A1525 SOLO

A1525 Solo – the most compact and affordable TMF unit with two phased array transducers and 3D v
...
isualization and analysis software in standard delivery set. A compact, ergonomic and easy to handheld Phased Array unit based on Total Focusing Method for easy-going imaging of inspection objects with two-dimensional and three-dimensional visualization and evaluation of inspection results.
>

Echomac® Small

Available with up to eight channels of electronics to detect and evaluate thickness, flaws and eccen
...
tricity, this UT tester is housed in a convenient, smaller cabinet. This instrument can be used in conjunction with bubbler or immersion tank systems, or with a test bench or in laboratory applications. The Echomac® Small is available in the FD4, FD6 or FD6A versions.
>

Ultrasonic Testing Immersion Tanks with Unmatched Scanning Features

TecScan’s non-destructive testing Ultrasonic Immersion Tanks & scanners are designed for high pe
...
rformance and demanding NDT testing applications. Our Scan3D™ line of High Precision Immersion Tanks are specifically designed for automated ultrasonic testing of complex composites parts used in aerospace and industrial applications.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window