AWS D1.1 versus Phased Array

Gentlemen,
Are the Acceptance Criteria of the table 6.2 and 6.3 ( statically and ciclically loaded) applicable to an inspection performed by PA system using sectorial or linear scan? The PA probes normally don't attempt to the characteristics established by AWS D1.1;
Thanks for any reply.
Manfred

 
 Reply 
 
Ed Ginzel
R & D, -
Materials Research Institute, Canada, Joined Nov 1998, 1307

Ed Ginzel

R & D, -
Materials Research Institute,
Canada,
Joined Nov 1998
1307
00:52 Sep-12-2009
Re: AWS D1.1 versus Phased Array
In Reply to Manfred Richter at 21:03 Sep-11-2009 (Opening).

Manfred:
As I read the AWS D1.1, the rules are written for manual UT using the equipment and procedures described in 6.20 and 6.22. Clearly these rules belong to the old traditional methods using monoelement probes and the many restrictions AWS has maintained over the past 4-5 decades. The acceptance criteria methods it uses are similarly based on the old conservative workmanship standards.
For some time now, in paragraph 6.20.2, provision has existed to deviate from these old and restrictive methods. 6.20.2 states "Variations in testing procedure, equipment and acceptance standards not included in Part F of Section 6 may be used with the approval of the Engineer."
Using phased-array techniques is already a deviation from Part F. The Equipment does not conform to the AWS "standard" expectations for manual equipment so the Engineer needs to approve its use. The next issue comes with how to anayse data. Phased-array data is not "initially" evaluated like the old manual UT using A-scans. Instead, a colour display is used from which the operator will identify areas of concern. In order that it be treated with consistancy for the range of inspection there SHOULD be a TCG used to assure the operator uses the same colour identification method for all flaws of concern. This means that (at least for the initial assessment) the AWS Rating method is not practical. The guidance in Appendix S COULD apply. Table S1 is "recommended" acceptance criteria for the methods that would use TCG...but the entire Appendix S is not considered part of AWS D1.1 and is provided only for information. Again, the table S1 is based on conservative workmanship criteria. Even so, its use would requrie Engineer approval.
Alternatively, a full engineering critical assessment could be run and other acceptance criteria submitted to the Engineer for approval.
It has been my experience however, that many engineers do not want to do the engineering. This requirement for the Engineer to "approve" all deviations from the old methods is perhaps the greatest impediment to advanced UT being used on AWS work. (IMHO)
Ed

 
 Reply 
 
Stan
NDT Inspector,
Canada, Joined Jan 2009, 31

Stan

NDT Inspector,
Canada,
Joined Jan 2009
31
16:12 Sep-14-2009
Re: AWS D1.1 versus Phased Array
In Reply to Ed Ginzel at 00:52 Sep-12-2009 .

Perhaps a way around the the problem of trying to asses indications to the criteria specified in AWS D1.1 while at the same time performing a Phased Array examination as may be allowed in Clause 6.20.2, would be to conduct a Phased Array examination to an ASME like procedure and to measure the length based upon the PA data, but to manually rate the defects using a standard AWS D1.1 rating procedure. Final defect assessment would be based on data from both methods, and when the location of the defects to be rated are known, the actual time spent rating them would not be that much extra.

 
 Reply 
 
Roger Duwe
NDT Inspector, API-510, 570, 653
MISTRAS, USA, Joined Jan 2009, 148

Roger Duwe

NDT Inspector, API-510, 570, 653
MISTRAS,
USA,
Joined Jan 2009
148
20:52 Sep-15-2009
Re: AWS D1.1 versus Phased Array
In Reply to Stan at 16:12 Sep-14-2009 .

As usual, Mr. Ginzel has cut to the heart of the problem. One possible suggestion, though:
You can point out to the structural Engineer that manual UT per D1.1 compares flaws to a 0.060 inch calibration hole, and that you can perform your PA calibration using the same 0.060" holes to build your TCG curve. This will give better correlation of deeper flaws to the calibration standard, instead of "add 2 dB for each inch of soundpath". A multipoint calibration with at least one point closer and one point farther away than the 'area of interest' will always be a more accurate calibration than a single-point calibration.

Further, if you show the Engineer the color pictures that a C-scan scope like the Omniscan can capture, you should have a customer for life. Personally, I have gotten tired of the scepticism I get at the end of a manual examination exam. I have nothing to show the Engineer but a chart listing indications, locations, and ratings. Some believe me, some remain sceptical until they get reports back from their welder that the flaws really were where I said they were, and what I said they were. "One picture vs 100 words"

The picture and data file is especially valuable to prove later that the indications judged as 'Acceptable" were indeed within the Code standards. On Bridge work especially, there is a lot of resistance to accepting any known defects, even when well within the Code limits.

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 897

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
897
04:12 Sep-16-2009
Re: AWS D1.1 versus Phased Array
In Reply to Roger Duwe at 20:52 Sep-15-2009 .

Roger,

I do agree with you, but it is not only in the bridge industry that acceptable indication are rejected by the client. We have the same situation with some of our clients. After seeing a few accidents happening 40 - 50 years after construction, can we blame the engineers?

 
 Reply 
 

Product Spotlight

Micro CT

nanoVoxel series has nano-scale resolution upto 500nm by using high voltage X-ray source (from 80-
...
300 kV) with micro/nano focal spot and highly sensitive flat panel detectors and unique Optical coupling detector.
>

Ultrasonic Probe Recharacterization Service

NDT Systems offers a comprehensive Aftercare and Recharacterization Service for all our ultrasonic
...
probes. The Recharacterization Service is fully compliant with International ASTM E1065 Standard Guide (and other applicable standards) and offers complete documentation, traceable to the ASTM E1065 Standard. For more details or to schedule Recharacterization Services contact ndtsales@ndtsystems.com
>

PAUT Probes

Typical Phased Array probes have frequencies between 1MHz and 20MHz and the number of wafers is 10
...
to 128. M2 Electronics offers customers conventionally ultrasound probes and the ability to provide high-precision Phased Array Ultrasound Probes of up to 256 wafers. We can also customize the probe for our customers to meet the specific application requirements of the user.
>

Immersion systems

ScanMaster ultrasonic immersion systems are designed for high throughput, multi shift operation in a
...
n industrial or lab environment. These fully integrated systems provide various scanning configurations and incorporate conventional and phased arrays technologies to support diverse applications, such as inspection of disks, bars, shafts, billets and plates. All of ScanMaster immersion systems are built from high accuracy scanning frames allowing for scanning of complex parts and include a multi-channel ultrasonic instrument with exceptional performance. The systems are approved by all major manufacturers for C-scan inspection of jet engine forged discs. Together with a comprehensive set of software modules these flexible series of systems provide the customer with the best price performance solutions.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window