where expertise comes together - since 1996 -

The Largest Open Access Portal of Nondestructive Testing (NDT)

Conference Proceedings, Articles, News, Exhibition, Forum, Network and more

where expertise comes together
- since 1996 -

TecScan Systems
We offer a complete line of NDT scanners, Immersion Tanks & Gantry systems which incorporate Ultrasonic, Phased Array & Eddy Current technologies.
689 views
Technical Discussions
Ramalingam
NDT Inspector,
QTech Instutitu of Nondistractive Testing, India, Joined Sep 2009, 1

Ramalingam

NDT Inspector,
QTech Instutitu of Nondistractive Testing,
India,
Joined Sep 2009
1
19:21 Sep-29-2009
what is mean by tandam echo

dear sir
i am work in forging company
some doutful question in UT what is mean by tandam echo

 
 Reply 
 
Peter Bruckner
NDT Inspector, NDT Manager
United Kingdom, Joined Jul 2008, 21

Peter Bruckner

NDT Inspector, NDT Manager
United Kingdom,
Joined Jul 2008
21
23:08 Sep-29-2009
Re: what is mean by tandam echo
In Reply to Ramalingam at 19:21 Sep-29-2009 (Opening).

Hi Ramalingam,
Usually tandem testing involves 2 identical shear wave probes facing the same direction on the surface of the bar a fixed distance apart. The distance between the probes is 1/2 skip, for 45 degree probe that is the thickness or diameter of the bar under test.
The only type of defect this will find is a planar one transverse to the beam at 1/2 thickness/diameter. The test standard usually consists of a flat bottomed hole drilled in the end of the bar.

I hope this is of some assistance.
Regards
Peter

 
 Reply 
 
Uli Mletzko
R & D, Retired
Germany, Joined Nov 1998, 89

Uli Mletzko

R & D, Retired
Germany,
Joined Nov 1998
89
11:44 Sep-30-2009
Re: what is mean by tandam echo
In Reply to Peter Bruckner at 23:08 Sep-29-2009 .

Hi Peter and Ramalingam,

the expression 'tandem' originates from a bicycle type for two persons, where the second person is sitting behind the first, both looking into the forward direction, and both pedaling.

In UT the distance between the two probes is not limited to 1/2 skip, but usually ist smaller than full skip. In testing of medium and heavy wall nuclear components, tandem is a standard system at least in Germany. We have arrangements of e.g. 3, 4 or 5 or more probes, each behind the other. Usually one probe acts as transmitter, the other ones as receivers. All sound pathes are reflecting on the surface opposite to the probe system, so in general you can inspect only components with parallel or coaxial surfaces. Using more than two probes will split the cross section to be inspected into several layers.

The presumed defects at tandem UT are not transverse to the sound beam, but perpendicular to the surface.

As far as I can remember, tandem UT was invented about 1970 by the German institutes and companies BAm and/or AEG, MAN and Siemens.

Regards
Uli Mletzko (retired, from MPA/University of Stuttgart/Germany)

 
 Reply 
 

Product Spotlight

Ultrasonic Squirter/Gantry System

TecScan’s NDT Ultrasonic Gantry Systems are industrial Squirter scanners designed for non-destru
...
ctive quality testing and raster scanning of large structures and parts. The Gantry Systems are usually composed of an Industrial Mechanical Scanner and a Control Room with System Workstation.
>

Varex Imaging Large Field of View (FOV) Digital Detector Arrays (DDAs)

A larger FOV DDA can reduce the space and volume of the X-ray inspection system on the factory floor
...
, enable faster scanning times, better throughput and better resolution images at a lower dose. Customers can also save time and money. With these benefits in mind, Varex Imaging has designed a family of large FOV detectors (4343HE, XRD 1611, 4343DX-I, 4343CT) for our industrial imaging customers.
>

TraiNDE UT

TraiNDE UT is a virtual tool associated with a signal database which simulates real inspection con
...
ditions for numerous applications (Type A/V1 block, DAC block, welds and plates).
>

Eddy Current inspection : RotoETscan Rotating Head

The rotating head RotoETscan detects the presence of longitudinal surface or sub surface defects a
...
t high speed. The rotating head is often installed directly on the production line. It is generally dedicated to the control of long products such as tubes, bars and wires, made of ferrous or non-ferrous material. It can also be used for inspection of small parts (billets).
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window