11:25 Oct-28-2009
ndt of cladding

Hi,
I have some experience with this. Usually the cladding has been used to build up a seal face before machining.

After machining we perform MPI or DPI checking for defects. Here we almost always find indications in the bond/fusion area between parent material and new cladding material. Both methods show indications. Usually a light machining will remove the indication but generally as its a seal area and been machined down this is not welcome by customer. You can actually see the fused line very well after machining.

Does anyone have experience on what is causing these indications?

Its an expensive process, welding, machining, checking etc so its difficult to just tell customers there is an rejectable indication and leave. Also difficult to leave indications in the item unidentified.



I have also done UT to check fusion between parent and weld materials sometimes but the item needs to be correct geometry for this.

I know wall thickness can be checked by different methods also.

 
 Reply 
 
Phil
NDT Inspector, Radiation Safety
BINDT, MIAQP, United Kingdom, Joined Mar 2009, 151

Phil

NDT Inspector, Radiation Safety
BINDT, MIAQP,
United Kingdom,
Joined Mar 2009
151
20:33 Nov-01-2009
Re: ndt of cladding
In Reply to anjafo at 11:25 Oct-28-2009 (Opening).

Hi Anjafo,

I have also done some work on what you call cladding, we have called Buttering, I am sure it is know by other names, I have done MT and PT, on it.

I would say lack of cleaning between runs, would leave slag behind and as so ypur indication

Regards,

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 869

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
869
22:02 Nov-03-2009
Re: ndt of cladding
In Reply to anjafo at 11:25 Oct-28-2009 (Opening).

Anjafo,

Were I used to work, we did this on Steam Generators tube sheets. We did sometimes have problems and it was always related to the welding process. But we didn't experience the type of defect that you are experiencing. I suggest maybe to have your welding engineer review the procedure and change some of the parameters such a rate of deposit and your amperage.

 
 Reply 
 
anjafo79
NDT Inspector
Norway, Joined Aug 2009, 204

anjafo79

NDT Inspector
Norway,
Joined Aug 2009
204
11:01 Nov-04-2009
Re: ndt of cladding
In Reply to Michel Couture at 22:02 Nov-03-2009 .

I am going to try get a picture of the next one we test. Will take a little time though.

Problem is indication appears with DPI also.

 
 Reply 
 

Product Spotlight

NEW - TD Focus-ScanRX

The NEW Next Generation Advanced UT platform, TD Focus ScanRX - Also available as a card stack solut
...
ion. Key Improvements 1. Data acquisition is significantly faster than current design 2. Better aesthetic – closely aligns with HandyScan RX 3. Improved IP rating (Target IP66) 4. Ruggedized housing 5. Connectors are protected from impact and ingress 6. Integrated stand and separate retractable handle easy to keep clean) 7. Touchscreen with ruggedized display glass 8. 3-Axis encoder input
>

Combination of Digital Image Correlation and Thermographic Measurements

The combination of measuring results from the digital image correlation (ARAMIS, DIC) and temperat
...
ure measuring data from infrared cameras permits the simultaneous analysis of the thermal and mechanical behavior of test specimens in the materials and components testing field.
>

NovaScope 6000

The all-digital Novascope 6000 is a portable, ultra-high precision thickness gauge for high-speed
...
thickness measurement. Novascope 6000 has unmatched capabilities and unique features including: •Superior Resolution with high contrast, high-speed color RF display •High pulser voltage •Real-time video output •Increased internal/external data storage •Programmable SetUp features •Battery & AC Powered
>

Lyft™: Pulsed Eddy Current Reinvented

PEC Reinvented—CUI Programs Redefined Corrosion under insulation (CUI) is possibly the greatest u
...
nresolved asset integrity problem in the industry. Current methods for measuring wall thickness with liftoff, without removing insulation, all have severe limitations. Eddyfi introduces Lyft — a reinvented, high-performance pulsed eddy current (PEC) solution. The patent- pending system features a state-of-the-art portable instrument, real- time C-scan imaging, fast data acquisition with grid-mapping and dynamic scanning modes, and flexibility with long cables. It can also scan through thick metal and insulation, as well as aluminum, stainless steel, and galvanized steel weather jackets. Who else but Eddyfi to reinvent an eddy current technique and redefine CUI programs. Got Lyft?
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window