NDT of turbine blades.

Dear all,

I want to perform the NDT of Turbine blades (with curved fir tree root) remvoved from rotor. Can any one comment on the following:

1) Which NDT technique is preferred to inspect the blades specifically root area. As per my knowledge Flourescent MPI (FMPI) is normally done
2) Which type of FMPI will give best results?
3) If we used Hand Yoke, will this be OK / sufficient or not?
4) If there is any other better way than yoke method, please giev brief detail.

Thanks & Regards
Azhar

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 868

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
868
03:20 Jan-28-2010
Re: NDT of turbine blades.
In Reply to Azhar Jamil at 23:38 Jan-27-2010 (Opening).

Azhar,

You are giving very little information as to what kind of turbine blades and where they are use. If the blades are used on aircraft engine, the engine manufacturer will already have an inspection procedure. For blades used in the power genenration industry, either the manufacturer will have an inspection procedure or the end users (engineers) will decide on an inspection procedure.

In Power Generation, I have seen Phased Array used with excellent results on turbine blade root and I'm sure other methods are used as well.

 
 Reply 
 
Alisher Tadjiev
NDT Inspector
Uzbekistan Airways Technics, Uzbekistan, Joined Mar 2005, 8

Alisher Tadjiev

NDT Inspector
Uzbekistan Airways Technics,
Uzbekistan,
Joined Mar 2005
8
05:29 Jan-28-2010
Re: NDT of turbine blades.
In Reply to Azhar Jamil at 23:38 Jan-27-2010 (Opening).

Hi Azhar
I'm agree with Mr.Couture - given info not enough to final decision
What kind of engines to be inspected?
For example - aircraft Pratt&Whitney 2000/4000 engine fan blades can be inspected via two ways
(acc. manufacturer documentation - Mr.Couture told about it before) - special Eddy Current probes with Reference Standard or Liquid Penetrant Inspection (Type I, Method C, Level IV).
By the way - all turbo engine rotating parts must be inspected by Level IV sensitivity penetrant (it is concerning penetrant inspection)
In case of Rolls Roys aircaraft engines with composite fan blades - fan blades must be inspected using special RR TAPTester (actually it is not TAP Tester - looks like composite bondmaster mode tester)

Regards

 
 Reply 
 
azhar jamil
azhar jamil
08:40 Jan-28-2010
Re: NDT of turbine blades.
In Reply to Azhar Jamil at 23:38 Jan-27-2010 (Opening).

Thanks. The blades are of steam turbine for Power Generation industry. Phase array technique is excedllent, but the blades to be inspected after removal from rotor i.e. each blade to be inspected separately.
There is no procedure from OEM is available

If any further details required let me know.

regards

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 868

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
868
15:38 Jan-28-2010
Re: NDT of turbine blades.
In Reply to azhar jamil at 08:40 Jan-28-2010 .

Azhar,

Since the blades are removed, phased array inspection would give better results. Their roots would be clean and you would eliminate the possibility of non-relevant indication in the root area cause by lubricant.

I guess what you can do is have some calibration pieces manufactured with artificial defects in the form of EDM notches of varying depth in the area of concern and then write your inspection procedure.

Good Luck!

 
 Reply 
 
aldo
Engineering
Italy, Joined Jan 2009, 39

aldo

Engineering
Italy,
Joined Jan 2009
39
15:50 Jan-28-2010
Re: NDT of turbine blades.
In Reply to Michel Couture at 15:38 Jan-28-2010 .

I speak by my exsperince in aeronautic industry in particular in maintenence activity and in production activity .. The typical NDT on blade in turbine are FPI with high sensibility (ID4) because are very critical part on engine... There are a lot applications with MPI because are sporadic case....
aldo

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 868

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
868
04:27 Jan-29-2010
Re: NDT of turbine blades.
In Reply to aldo at 15:50 Jan-28-2010 .

Aldo,

I totally concur with you regarding aircraft turbine engine. I have as well done many FPI Level 4 on Fan Blades to detect cracking resulting from FOD (Foreign Object Damage) injestion.

I have also personally done some UT inspection of root cracking on Fan Blades of the Pratt & Whitney JT-3D which were propulsing the Boeing 707 using UT Surface Wave.

The advice Azhar is seeking is in regards to blade root inspection of turbine used in Power Generation.

 
 Reply 
 
Rafid O. Lopez
, NDT Level 3
Mexico, Joined Jan 2010, 81

Rafid O. Lopez

, NDT Level 3
Mexico,
Joined Jan 2010
81
16:03 Jan-30-2010
Re: NDT of turbine blades.
In Reply to Michel Couture at 04:27 Jan-29-2010 .

Hello

We work with P & W (JT8D-200), GE (CFM-56 model 5 and 7) all aircraft engines and all inspection of blades (with curved fir tree root) are with FPI some with Type 1, Method A Level 3 or Type 1, Method D Level 4.

For your inspection i think that is more easy to do an inspection with FPI.

Is a commentary.

Best regards.

Rafid

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 868

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
868
04:15 Jan-31-2010
Re: NDT of turbine blades.
In Reply to Rafid O. Lopez at 16:03 Jan-30-2010 .

Rafid,

In a way I must agree with you. FPI is much simpler, but other methods like PAUT for exemple provide on thing FPI can't and that is a permanent record of the inspection. In my opinion, it also provide a more sensitive inspection because it is less suceptible to surface dirt. I mean, blade cleanliness is not as rigurous as FPI.

 
 Reply 
 

Product Spotlight

TESTD-PT SYSTEM

Pulse thermography is a non-contact test method that is ideal for the characterization of thin fil
...
ms and coatings or the detection of defects. With a remarquable short test time and a high detection sensitivity, the Telops TESTD-PT is the perfect tool for non- destructive testing. With such high frame rates, it is even possible to investigate highly conductive or diffusive materials.
>

Immersion systems

ScanMaster ultrasonic immersion systems are designed for high throughput, multi shift operation in a
...
n industrial or lab environment. These fully integrated systems provide various scanning configurations and incorporate conventional and phased arrays technologies to support diverse applications, such as inspection of disks, bars, shafts, billets and plates. All of ScanMaster immersion systems are built from high accuracy scanning frames allowing for scanning of complex parts and include a multi-channel ultrasonic instrument with exceptional performance. The systems are approved by all major manufacturers for C-scan inspection of jet engine forged discs. Together with a comprehensive set of software modules these flexible series of systems provide the customer with the best price performance solutions.
>

NDT Master Lecturer

In the program both university professors and practitioners will give lectures, which guarantees the
...
oretical depth and practical inside. Academic Director: Prof. Dr. Christian Boller
The following lecturers are not complete: Prof. Tadeusz Stepinski, Prof. Wieslaw Staszewski, Prof. Frank Walther, Prof. Giovanni Bruno, Prof. Gerd Dobmann, Prof. Philippe Guy
>

MIZ®-21C: Truly Affordable Eddy Current Handheld with Surface Array Capability

Introducing MIZ-21C, the first truly affordable handheld eddy current instrument with surface array
...
capabilities. MIZ-21C can deliver fast, accurate inspections in demanding NDT applications including aerospace, oil and gas, manufacturing, and power generation. The surface array solution can reduce inspection time by up to 95% compared to traditional handheld pencil probes. The ergonomic design, long battery life, and intuitive touchscreen mean you can inspect more areas faster than ever without fatigue.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window