Dear all,

I want to perform the NDT of Turbine blades (with curved fir tree root) remvoved from rotor. Can any one comment on the following:

1) Which NDT technique is preferred to inspect the blades specifically root area. As per my knowledge Flourescent MPI (FMPI) is normally done
2) Which type of FMPI will give best results?
3) If we used Hand Yoke, will this be OK / sufficient or not?
4) If there is any other better way than yoke method, please giev brief detail.

Thanks & Regards
Azhar

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 868

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
868
03:20 Jan-28-2010
Re: NDT of turbine blades.
In Reply to Azhar Jamil at 23:38 Jan-27-2010 (Opening).

Azhar,

You are giving very little information as to what kind of turbine blades and where they are use. If the blades are used on aircraft engine, the engine manufacturer will already have an inspection procedure. For blades used in the power genenration industry, either the manufacturer will have an inspection procedure or the end users (engineers) will decide on an inspection procedure.

In Power Generation, I have seen Phased Array used with excellent results on turbine blade root and I'm sure other methods are used as well.

 
 Reply 
 
Alisher Tadjiev
NDT Inspector
Uzbekistan Airways Technics, Uzbekistan, Joined Mar 2005, 8

Alisher Tadjiev

NDT Inspector
Uzbekistan Airways Technics,
Uzbekistan,
Joined Mar 2005
8
05:29 Jan-28-2010
Re: NDT of turbine blades.
In Reply to Azhar Jamil at 23:38 Jan-27-2010 (Opening).

Hi Azhar
I'm agree with Mr.Couture - given info not enough to final decision
What kind of engines to be inspected?
For example - aircraft Pratt&Whitney 2000/4000 engine fan blades can be inspected via two ways
(acc. manufacturer documentation - Mr.Couture told about it before) - special Eddy Current probes with Reference Standard or Liquid Penetrant Inspection (Type I, Method C, Level IV).
By the way - all turbo engine rotating parts must be inspected by Level IV sensitivity penetrant (it is concerning penetrant inspection)
In case of Rolls Roys aircaraft engines with composite fan blades - fan blades must be inspected using special RR TAPTester (actually it is not TAP Tester - looks like composite bondmaster mode tester)

Regards

 
 Reply 
 
azhar jamil
azhar jamil
08:40 Jan-28-2010
Re: NDT of turbine blades.
In Reply to Azhar Jamil at 23:38 Jan-27-2010 (Opening).

Thanks. The blades are of steam turbine for Power Generation industry. Phase array technique is excedllent, but the blades to be inspected after removal from rotor i.e. each blade to be inspected separately.
There is no procedure from OEM is available

If any further details required let me know.

regards

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 868

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
868
15:38 Jan-28-2010
Re: NDT of turbine blades.
In Reply to azhar jamil at 08:40 Jan-28-2010 .

Azhar,

Since the blades are removed, phased array inspection would give better results. Their roots would be clean and you would eliminate the possibility of non-relevant indication in the root area cause by lubricant.

I guess what you can do is have some calibration pieces manufactured with artificial defects in the form of EDM notches of varying depth in the area of concern and then write your inspection procedure.

Good Luck!

 
 Reply 
 
aldo
Engineering
Italy, Joined Jan 2009, 39

aldo

Engineering
Italy,
Joined Jan 2009
39
15:50 Jan-28-2010
Re: NDT of turbine blades.
In Reply to Michel Couture at 15:38 Jan-28-2010 .

I speak by my exsperince in aeronautic industry in particular in maintenence activity and in production activity .. The typical NDT on blade in turbine are FPI with high sensibility (ID4) because are very critical part on engine... There are a lot applications with MPI because are sporadic case....
aldo

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 868

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
868
04:27 Jan-29-2010
Re: NDT of turbine blades.
In Reply to aldo at 15:50 Jan-28-2010 .

Aldo,

I totally concur with you regarding aircraft turbine engine. I have as well done many FPI Level 4 on Fan Blades to detect cracking resulting from FOD (Foreign Object Damage) injestion.

I have also personally done some UT inspection of root cracking on Fan Blades of the Pratt & Whitney JT-3D which were propulsing the Boeing 707 using UT Surface Wave.

The advice Azhar is seeking is in regards to blade root inspection of turbine used in Power Generation.

 
 Reply 
 
Rafid O. Lopez
, NDT Level 3
Mexico, Joined Jan 2010, 81

Rafid O. Lopez

, NDT Level 3
Mexico,
Joined Jan 2010
81
16:03 Jan-30-2010
Re: NDT of turbine blades.
In Reply to Michel Couture at 04:27 Jan-29-2010 .

Hello

We work with P & W (JT8D-200), GE (CFM-56 model 5 and 7) all aircraft engines and all inspection of blades (with curved fir tree root) are with FPI some with Type 1, Method A Level 3 or Type 1, Method D Level 4.

For your inspection i think that is more easy to do an inspection with FPI.

Is a commentary.

Best regards.

Rafid

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 868

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
868
04:15 Jan-31-2010
Re: NDT of turbine blades.
In Reply to Rafid O. Lopez at 16:03 Jan-30-2010 .

Rafid,

In a way I must agree with you. FPI is much simpler, but other methods like PAUT for exemple provide on thing FPI can't and that is a permanent record of the inspection. In my opinion, it also provide a more sensitive inspection because it is less suceptible to surface dirt. I mean, blade cleanliness is not as rigurous as FPI.

 
 Reply 
 

Product Spotlight

Varex Imaging Large Field of View (FOV) Digital Detector Arrays (DDAs)

A larger FOV DDA can reduce the space and volume of the X-ray inspection system on the factory floor
...
, enable faster scanning times, better throughput and better resolution images at a lower dose. Customers can also save time and money. With these benefits in mind, Varex Imaging has designed a family of large FOV detectors (4343HE, XRD 1611, 4343DX-I, 4343CT) for our industrial imaging customers.
>

Combination of Digital Image Correlation and Thermographic Measurements

The combination of measuring results from the digital image correlation (ARAMIS, DIC) and temperat
...
ure measuring data from infrared cameras permits the simultaneous analysis of the thermal and mechanical behavior of test specimens in the materials and components testing field.
>

Wireless TOFD scanner

Quick, accurate and highly reproducible welds testing. The System operates wirelessly and is compat
...
ible with any type of Windows based Laptop, Desktop or Tablet.
>

Semi-Automated Phased Array Immersion System for Small Composite Parts

Turn-key semi-automated system as an improved and affordable solution for inspection of small comp
...
osite parts. Includes support table, immersion tank, scanner, PA instrument, PC, Analysis software, database, wedge management and other options.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window