basemetal indications

Level 2 ut tech finding several non-lamilar indications in the basemetal outside of the heat effected zone. Scanning to aws D1.1 with manual sherwave and can not find accept/reject criteria for this. The code talks about lamilar indications but there is no info on n on lamilar. They can't be rejected with a straight beam transducer.

 
 Reply 
 
Michel Couture
NDT Inspector,
consultant, Canada, Joined Sep 2006, 897

Michel Couture

NDT Inspector,
consultant,
Canada,
Joined Sep 2006
897
13:19 Feb-23-2010
Re: basemetal indications
In Reply to ut tech at 08:53 Feb-23-2010 (Opening).

It would appear the metal is of pour quality. What I suggest is to find the ASTM stardard pertaining to the metal and quality you or your customer is suppose to have and see what the acceptance criterias are.

 
 Reply 
 
Jon Wallis
NDT Inspector, -
Netherlands, Joined Feb 2010, 626

Jon Wallis

NDT Inspector, -
Netherlands,
Joined Feb 2010
626
09:41 Feb-24-2010
Re: basemetal indications
In Reply to ut tech at 08:53 Feb-23-2010 (Opening).

The problem is that when you are conducting a weld examination, the object of the examination is to check for weld defects. In order to do this satisfactorily you have to scan through the base metal with angle probes (search units). The reason for the base metal examination, prior to the weld examination, is to ensure that the base material is homogeneous and therefore allows the ultrasound to pass through.

So, the base metal examination is only to determine whether there are inhomogenities present that will interfere with the weld examination. This means in practice, if the indications are large enough to interfere with the weld examination, you report this to your client. Now, he won't be very happy because 1. his weld hasn't been examined. 2. His plate material might be useless.

The next step would be to carry out a lamination examination of the plate material and this examination uses a different code which does include accept/reject criteria.

Horses for courses!

 
 Reply 
 
ut tech
ut tech
10:32 Feb-24-2010
Re: basemetal indications
In Reply to Jon Wallis at 09:41 Feb-24-2010 .

The problem is that the indications do not show up with the lam scan. They are only detected with an angle beam shear wave transducer. The material is relativaly thin when looking at AWS D1.1 so the alternative scans dont really help either. The problem that we need to solve is wether we reject them and scrap or repair the areas or if we provide as much info about them as possible and leave them alone. They are also not rejectable to ASTM 578 (I believe that is what we needed to look at but dont have the info in front of me rt now).

 
 Reply 
 
Jon Wallis
NDT Inspector, -
Netherlands, Joined Feb 2010, 626

Jon Wallis

NDT Inspector, -
Netherlands,
Joined Feb 2010
626
12:44 Feb-24-2010
Re: basemetal indications
In Reply to ut tech at 10:32 Feb-24-2010 .

Ok, I should have read your original question better, sorry.

It looks like you have randomly orientated inclusions in the base metal material. If the code requires you to examine only with a straight beam (sorry I don't have the AWS code at hand - not much call for it in my sphere of ops.) then stick to the code for reporting purposes and report verbally to the client the problem.

Maybe you need to get a sample of the plate analysed or speak with the construction engineers as to fitness. Are the indications surface breaking? If so, it may be cracking!!!

 
 Reply 
 
ut tech
ut tech
02:53 Feb-25-2010
Re: basemetal indications
In Reply to Jon Wallis at 12:44 Feb-24-2010 .

They aren't surface breaking and not crack. Maybe silica builups but have a rejectable rating but are/out of the weld an d haz.

 
 Reply 
 

Product Spotlight

Immersion systems

ScanMaster ultrasonic immersion systems are designed for high throughput, multi shift operation in a
...
n industrial or lab environment. These fully integrated systems provide various scanning configurations and incorporate conventional and phased arrays technologies to support diverse applications, such as inspection of disks, bars, shafts, billets and plates. All of ScanMaster immersion systems are built from high accuracy scanning frames allowing for scanning of complex parts and include a multi-channel ultrasonic instrument with exceptional performance. The systems are approved by all major manufacturers for C-scan inspection of jet engine forged discs. Together with a comprehensive set of software modules these flexible series of systems provide the customer with the best price performance solutions.
>

Customized Probes and Transducers

With a strong development department and our own piezocomposite production, we accompany you from th
...
e first product idea to serial production. Our scientists are continuously researching new methods in the field of ultrasonic measurement technology. The progress achieved enables us to offer you optimal solutions.
>

Robotic laser shearography enables 100% inspection of complex, flight-critical composite structures

An article in “Composites World Magazine” showcases Non Destructive Testing of aero-structures
...
with Laser Shearography. Over the years Dantec Dynamics has supplied many solutions for the aerospace industry. Referring to specific customer projects several of these cases are examined to outline the advantages of using Laser Shearography for automated defect detection.
>

OPBOX with standard software is able to do all types of inspections and measurements: flaw detection in welds and materials, scanning of objects, testing composite materials, forged and moulded pieces, many UT inspections, measurements of properties of ma

Typical applications: UT measurements with pulse technique, Measurement of thicknesses also at hig
...
h temperatures, Measurements of properties of materials, including fluids and gases We are delivering a standard version of the software (for any Microsoft Windows up to 10 x64 with Microsoft Hardware certification report Approved) and for special needs: SDK with ready to use examples for LabView, MATLAB x64, C++ wrapper for dll, Python and Linux., and also low-level description of how to control our devices directly from any USB tools
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window