Nandesh Kumar A
14:21 Feb-28-2010
Can anybody explain me for ISO 13847 ?

One of our code (ISO 13847 ) says the following.

"The total area, when projected radially through the weld, shall not exceed 2% of the projected weld area in the radiograph. The area shall be the length the weld affected by the porosity (with a minimum length of 150 mm ) times the maximum width of the weld."

The above criterion is in order to evaluate porosity on a radiograph. Now I've a uniformly distributed porosity of upto 45 mm length. The total length of the weld is 192 cm (24 inch OD, pipeline )Can anybody explain me (if possible with a sketch) how to proceed with it?

Replies are highly appreciated.

Nandesh Kumar

 
 Reply 
 
Nigel Armstrong
Engineering, - Specialist services
United Kingdom, Joined Oct 2000, 1096

Nigel Armstrong

Engineering, - Specialist services
United Kingdom,
Joined Oct 2000
1096
15:09 Mar-01-2010
Re: Can anybody explain me for ISO 13847 ?
In Reply to Nandesh Kumar A at 14:21 Feb-28-2010 (Opening).

Nandesh

If the weld length affected by porosity is 45mm, this is less than 150mm and so you must use the default 150mm figure. Multiply this by the maximum width of the weld in the affected region and then multiply by 0,02 (2%). Say the weld width is 25mm: 150mm x 25mm x 0,02 = 75 sq mm. Measure and add together all pore diameters in the affected region, multiply the total by pi. If the calcualted figure is less than your previous calculation (75 sq mm in my example) then the area is accpetable. Greater pore area sum total = rejectable.

Hope this helps

 
 Reply 
 
Nandesh
Nandesh
05:33 Mar-02-2010
Re: Can anybody explain me for ISO 13847 ?
In Reply to Nigel Armstrong at 15:09 Mar-01-2010 .

Thanks Nigel...but can ypu please explain me whats the terms " projected radially" and " projected weld area " in my post?
Regards,

 
 Reply 
 
Nigel Armstrong
Engineering, - Specialist services
United Kingdom, Joined Oct 2000, 1096

Nigel Armstrong

Engineering, - Specialist services
United Kingdom,
Joined Oct 2000
1096
06:34 Mar-02-2010
Re: Can anybody explain me for ISO 13847 ?
In Reply to Nandesh at 05:33 Mar-02-2010 .

Nandesh

The use of "projected" radially and weld area is to maintain proportionality with regard to image magnification. If the set-up used has a low ratio between source-to-object distance and material thickness, differential magnification will enlarge a source-side pore more than a film-side pore.

Assuming you used a panoramic exposure on a 24" sch 40 pipe (wt = 0,375") then differential magnification is not a problem you need worry about.

Hope that helps

Nigel

 
 Reply 
 
Muhammad
Muhammad
13:08 Feb-08-2014
Re: Can anybody explain me for ISO 13847 ?
In Reply to Nigel Armstrong at 15:09 Mar-01-2010 .

Sir can you please help me to understand below clause of my project spec.
"The distribution of scattered porosity is such that when projected radially through the weld the total area of porosity exceeds 1% of any 600mm Sq of projected weld metal."
Thanks in advance

 
 Reply 
 

Product Spotlight

NOVO Armor 15 & NOVO Armor 22

The Armor Kit Contains the NOVO Armor, which provides additional mechanical protection to the NOVO 1
...
5WN & NOVO 22WN Detectors, the Armor Stand and a traveling soft cover. - Newest shock absorbent technology case - Water resistant design - Supports wired & wireless communication - Multiple positioning options - Tripod connection using the Built-in 1/4” threads - Simple Detector battery replacement
>

GEKKO - Portable Phased Array Testing with TFM in Real-Time

The portable phased array testing system GEKKO provides 64 parallel test channels. On creating testi
...
ng parameters the operator is assisted by the CIVA software. Due to its modular set-up the GEKKO instrument is suitable for operators of all skill levels.
>

Wireless TOFD scanner

Quick, accurate and highly reproducible welds testing. The System operates wirelessly and is compat
...
ible with any type of Windows based Laptop, Desktop or Tablet.
>

VOGT Ultrasonics awarded innovation champion

Let go of the old and try something new. VOGT convinced the jury in the 27th round of the TOP 100
...
innovation competition. Our team is very pleased to officially belong to the TOP 100 in Germany!
>