Can anybody explain me for ISO 13847 ?

One of our code (ISO 13847 ) says the following.

"The total area, when projected radially through the weld, shall not exceed 2% of the projected weld area in the radiograph. The area shall be the length the weld affected by the porosity (with a minimum length of 150 mm ) times the maximum width of the weld."

The above criterion is in order to evaluate porosity on a radiograph. Now I've a uniformly distributed porosity of upto 45 mm length. The total length of the weld is 192 cm (24 inch OD, pipeline )Can anybody explain me (if possible with a sketch) how to proceed with it?

Replies are highly appreciated.

Nandesh Kumar

 
 Reply 
 
Nigel Armstrong
Engineering, - Specialist services
United Kingdom, Joined Oct 2000, 1096

Nigel Armstrong

Engineering, - Specialist services
United Kingdom,
Joined Oct 2000
1096
15:09 Mar-01-2010
Re: Can anybody explain me for ISO 13847 ?
In Reply to Nandesh Kumar A at 14:21 Feb-28-2010 (Opening).

Nandesh

If the weld length affected by porosity is 45mm, this is less than 150mm and so you must use the default 150mm figure. Multiply this by the maximum width of the weld in the affected region and then multiply by 0,02 (2%). Say the weld width is 25mm: 150mm x 25mm x 0,02 = 75 sq mm. Measure and add together all pore diameters in the affected region, multiply the total by pi. If the calcualted figure is less than your previous calculation (75 sq mm in my example) then the area is accpetable. Greater pore area sum total = rejectable.

Hope this helps

 
 Reply 
 
Nandesh
Nandesh
05:33 Mar-02-2010
Re: Can anybody explain me for ISO 13847 ?
In Reply to Nigel Armstrong at 15:09 Mar-01-2010 .

Thanks Nigel...but can ypu please explain me whats the terms " projected radially" and " projected weld area " in my post?
Regards,

 
 Reply 
 
Nigel Armstrong
Engineering, - Specialist services
United Kingdom, Joined Oct 2000, 1096

Nigel Armstrong

Engineering, - Specialist services
United Kingdom,
Joined Oct 2000
1096
06:34 Mar-02-2010
Re: Can anybody explain me for ISO 13847 ?
In Reply to Nandesh at 05:33 Mar-02-2010 .

Nandesh

The use of "projected" radially and weld area is to maintain proportionality with regard to image magnification. If the set-up used has a low ratio between source-to-object distance and material thickness, differential magnification will enlarge a source-side pore more than a film-side pore.

Assuming you used a panoramic exposure on a 24" sch 40 pipe (wt = 0,375") then differential magnification is not a problem you need worry about.

Hope that helps

Nigel

 
 Reply 
 
Muhammad
Muhammad
13:08 Feb-08-2014
Re: Can anybody explain me for ISO 13847 ?
In Reply to Nigel Armstrong at 15:09 Mar-01-2010 .

Sir can you please help me to understand below clause of my project spec.
"The distribution of scattered porosity is such that when projected radially through the weld the total area of porosity exceeds 1% of any 600mm Sq of projected weld metal."
Thanks in advance

 
 Reply 
 

Product Spotlight

On Demand Webinar: Using Eddy Current Array for Large Areas in Place of Magnetic Particle and Liquid Penetrant Testing

New on-demand webinar on the use of eddy current array (ECA) technology in lieu of liquid penetrant
...
testing (PT) and magnetic particle testing (MT) for large area screenings. The webinar includes an introduction to the technologies with advantages and disadvantages of each. Side by side examples are discussed including aircraft stringers, engine blades, forgings, weld plates & more. View it today.
>

SITEX CPSERIES

Teledyne ICM’s CPSERIES has been designed with a view to revolutionizing the handling and perfor
...
mances of portable X-Ray sets. Despite having managed to halve the weight of similar portable X-Ray generators available on the market (while continuing to provide the same power output), the SITEX CPSERIES generators feature a shutter, a laser pointer, a beryllium window, an aluminum filter and two integrated diaphragms (customized sizes are available upon request). Without compromising the robustness and reliability for which ICM products are renowned, the small size and light weight of the SITEX CPSERIES will radically change the way that you perform your RT inspections. And you will see a positive impact in terms of both quality and return on investment (ROI).
>

NOVO Armor 15 & NOVO Armor 22

The Armor Kit Contains the NOVO Armor, which provides additional mechanical protection to the NOVO 1
...
5WN & NOVO 22WN Detectors, the Armor Stand and a traveling soft cover. - Newest shock absorbent technology case - Water resistant design - Supports wired & wireless communication - Multiple positioning options - Tripod connection using the Built-in 1/4” threads - Simple Detector battery replacement
>

NDTkit RT

NDTkit RT, TESTIA's Digital Radiography software The NDTkit product line software for X-ray analysi
...
s. NDTkit RT is a software benefiting from the Ultis kernel which is dedicated to radiographic image analysis. It offers a set of tools and filtering processes to assist RT operators in finding relevant flaws.
>