UT on duplex steel casting

DEar All,
i have one duplex steel casting which thickness is 100 mm.
can anyone advice me how test to the casting ?
any special technique like PA or TOFD will help?

appreciate your response....
regards
rama

1    
 
 Reply 
 
S.V.Swamy
Engineering, - Material Testing Inspection & Quality Control
Retired from Nuclear Fuel Complex , India, Joined Feb 2001, 787

S.V.Swamy

Engineering, - Material Testing Inspection & Quality Control
Retired from Nuclear Fuel Complex ,
India,
Joined Feb 2001
787
15:37 Mar-06-2010
Re: UT on duplex steel casting
In Reply to ram at 11:48 Mar-06-2010 (Opening).

Dear Rama,

Depending on the applications, many castings are produced to some national or international standards. The standard and or the supplementary requirements specified by the designer, customer would specify the inspection requirements. Before a casting is made, a production and quality assurance manual / procedures would have been prepared.

If you are a researcher and are trying to investigate the casting, you can try ultrasonic testing and radiography, apart from penetrant testing.

The acceptance criteria would again be dependent on the application.

Regards

Swamy

    
 
 Reply 
 
rama
NDT Inspector, -
Kuwait, Joined Jan 2010, 13

rama

NDT Inspector, -
Kuwait,
Joined Jan 2010
13
05:30 Mar-07-2010
Re: UT on duplex steel casting
In Reply to S.V.Swamy at 15:37 Mar-06-2010 .

Dear Swamy ,
thank you vry much....but ....
what's is the effect of UT on DUPLEX STEEL CATING?
and is there any real advantage of Phassed Arry or TOFD over conventional UT?
if u using conventional UT is there any spl transducer is req?

    
 
 Reply 
 
Nigel Armstrong
Engineering, - Specialist services
United Kingdom, Joined Oct 2000, 1096

Nigel Armstrong

Engineering, - Specialist services
United Kingdom,
Joined Oct 2000
1096
09:54 Mar-07-2010
Re: UT on duplex steel casting
In Reply to rama at 05:30 Mar-07-2010 .

Well Ram at 100mm thickness I can imagine slow cooling, grain growth with all the concomitant ills (as far as UT) that entails. Scatter, beam-bending, noise requiring low frequency compression wave small diameter probe (to maximise beam-spread coverage). Your probe supplier may have wide coverage probes.

Your will need a castings expert to tell you sites of potential defects if you want to focus on those areas.

    
 
 Reply 
 
S.V.Swamy
Engineering, - Material Testing Inspection & Quality Control
Retired from Nuclear Fuel Complex , India, Joined Feb 2001, 787

S.V.Swamy

Engineering, - Material Testing Inspection & Quality Control
Retired from Nuclear Fuel Complex ,
India,
Joined Feb 2001
787
12:59 Mar-08-2010
Re: UT on duplex steel casting
In Reply to rama at 05:30 Mar-07-2010 .

Dear Rama,

In addition to what Nigel Armstrong wrote, I would like to add that without knowing more about the casting details and the defect level that is being attempted, we cannot advise specific details. Phased Array or TOFD have their specific advantages over conventional UT but unless you are just playing around with the casting and also have access to all such instruments in house, it would be advisable to exhaust the power of conventional NDT techniques.

Unless you come up with specific details of the casting and the applicable specifications, our advice is bound to be generalistic.

Regards

Swamy

    
 
 Reply 
 

Product Spotlight

TESTD-PT SYSTEM

Pulse thermography is a non-contact test method that is ideal for the characterization of thin fil
...
ms and coatings or the detection of defects. With a remarquable short test time and a high detection sensitivity, the Telops TESTD-PT is the perfect tool for non- destructive testing. With such high frame rates, it is even possible to investigate highly conductive or diffusive materials.
>

ISONIC 3510

Very Powerful Superior Performance Extremely Portable Smart Phased Array Ultrasonic Flaw Detector an
...
d Recorder with 2 Conventional UT and TOFD Channels uniquely combines PA, single- and multi-channel conventional UT, and TOFD modalities providing 100% raw data recording and imaging. Suitable for all kinds of every-day ultrasonic inspections
>

Combination of Digital Image Correlation and Thermographic Measurements

The combination of measuring results from the digital image correlation (ARAMIS, DIC) and temperat
...
ure measuring data from infrared cameras permits the simultaneous analysis of the thermal and mechanical behavior of test specimens in the materials and components testing field.
>

HARDNESS TESTER TKM-459CE combi

TKM-459CE combi applies 2 methods of hardness control: UCI and Leeb. It provides high-accuracy tes
...
ting of metals and alloys as well as items of different sizes and configurations, their hardened layers and galvanic coatings. Device represents results in HB, HRC, HV and others. Shock-, dust- and water-proof housing with intuitive software make this gauge easy to use in all working conditions.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window