where expertise comes together - since 1996 -

The Largest Open Access Portal of Nondestructive Testing (NDT)

Conference Proceedings, Articles, News, Exhibition, Forum, Network and more

where expertise comes together
- since 1996 -

Vallen-Systeme GmbH
The Acoustic Emission Company! Since 1987 Vallen stands for competence and continuity in AE and for reliable business cooperation and support.
2928 views
Technical Discussions
saranjee
Engineering, NDT Engineer
Malaysia, Joined Apr 2010, 24

saranjee

Engineering, NDT Engineer
Malaysia,
Joined Apr 2010
24
15:41 May-20-2010
ASME 2235-9

Dear Sir,

I did below calculation according to ASME 2235-9 for thickness 50mm. Please correct me if I am wrong.


1) Surface indication length 30mm, Height 4mm

a) Aspect Ratio = a/l= 4/30 = 0.13

b) a/t = 4/50=0.08



2) Subsurface indication length 25mm, Height 3mm

a) Aspect Ratio = a/2/l= 3/2/25 = 0.06

b) a/2/t = 3/2/50 = 0.03


For all subsurface indication, I divide the height of the indication by 2 and can anyone let me know which sentence mentioning that we need to divide the subsurface indication height by 2 in ASME 2235-9 because I couldn’t find any information about the calculation. Thanks in advance.

 
 Reply 
 
Stan
NDT Inspector,
Canada, Joined Jan 2009, 31

Stan

NDT Inspector,
Canada,
Joined Jan 2009
31
16:06 May-20-2010
Re: ASME 2235-9
In Reply to saranjee at 15:41 May-20-2010 (Opening).

CC2235-9 Fig 1 page 4 gives a diagram showing how to measure defect height for surface and subsurface flaws.
(i)(3)(b) is the clause that defines the use of a and 2a.
Don't forget to read (i)(4)(a) for surface connected flaws, last sentence. A 30 mm long surface connected flaw will not be allowed by any Construction Codes that I can think of.

 
 Reply 
 
Ed Ginzel
R & D, -
Materials Research Institute, Canada, Joined Nov 1998, 1285

Ed Ginzel

R & D, -
Materials Research Institute,
Canada,
Joined Nov 1998
1285
16:54 May-20-2010
Re: ASME 2235-9
In Reply to saranjee at 15:41 May-20-2010 (Opening).

Sarangee
You have calculated "a". As per the normal protocol of fracture mechanics, the height of a subsurface flaw is 2a. Therefore you would calculate the "a" for the subsurface flaw and then double that value.
If for your surface flaw your a/t is 4/50 then the maximum length allowed is that which makes a/l=0.4 or about 10mm.
For the subsurface flaw 3mm high that means 2a=3mm and "a" is 1.5 so your a/t is 0.03. There is no limit on the aspect ratio here so if it is a recordable indication your limiting factor is 4t. There is no sentence in CC2235 saying to divide by 2 because it is clear from the Figures that the height you measure for the subsurface flaw is twice the value you are to use in the computations.

 
 Reply 
 
Dao Huu Xuan
Other,
Vietnam, Joined Feb 2007, 18

Dao Huu Xuan

Other,
Vietnam,
Joined Feb 2007
18
17:23 May-20-2010
Re: ASME 2235-9
In Reply to saranjee at 15:41 May-20-2010 (Opening).

Dear Saranjee,

As my calculation:

Firstly, we should calculate indication height "a" from given a/t ratio. Second, calculate indication length "l" from a/l ratio. Then you get the indication length in correspondent to the indication height.

This table shows surface flaw acceptance criteria for t=50mm

t a/t Surf a a/l l
50.00 0.031 1.55 0.00 any
0.033 1.65 0.05 33.00
0.036 1.80 0.10 18.00
0.041 2.05 0.15 13.67
0.047 2.35 0.20 11.75
0.055 2.75 0.25 11.00
0.064 3.20 0.30 10.67
0.074 3.70 0.35 10.57
0.083 4.15 0.40 10.38
0.085 4.25 0.45 9.44
0.087 4.35 0.50 8.70

So, if indication height is 4mm, the permitable length is 10.38 mm (lesser of 10.38 and 10.57). And also, if indication length is 30mm, the permitable height is 1.65 mm.
If the indication height 1.55mm or less, then indication is accepted with regardless the length.

For subsurface flaw, calculation also similar:

t a/t Sub a a/l l
50.00 0.034 1.70 0.00 any
0.038 1.90 0.05 38.00
0.043 2.15 0.10 21.50
0.049 2.45 0.15 16.33
0.057 2.85 0.20 14.25
0.066 3.30 0.25 13.20
0.078 3.90 0.30 13.00
0.090 4.50 0.35 12.86
0.105 5.25 0.40 13.13
0.123 6.15 0.45 13.67
0.143 7.15 0.50 14.30


thanks

 
 Reply 
 
saranjee
Engineering, NDT Engineer
Malaysia, Joined Apr 2010, 24

saranjee

Engineering, NDT Engineer
Malaysia,
Joined Apr 2010
24
08:36 May-22-2010
Re: ASME 2235-9
In Reply to Ed Ginzel at 16:54 May-20-2010 .

Dear Sir,

The table 2 only gave us aspect ratio until 0.50. if my aspect ratio more then 0.50 what i should do?Do i need to reject all the indication above 0.50?Did the code case mention anything about this?Thanks for advance.

 
 Reply 
 
Oliviero
NDT Inspector,
Quality Control srl, Italy, Joined Oct 2008, 414

Oliviero

NDT Inspector,
Quality Control srl,
Italy,
Joined Oct 2008
414
13:39 May-22-2010
Re: ASME 2235-9
In Reply to saranjee at 08:36 May-22-2010 .

Dear Saranjee,

the Code Case at point (c) states that "Flaw size shall be not larger than the flaw in Table 1, 2 or 3 for the thickness to be examined".
This means that any flaw with an "a/l" aspect ratio greater than included in Table 2 is rejectable.
This is the formal point of view.

Technically you can reach the same answer thinking to what means an aspect ratio "a/l" 0,50.
Since it means that the flaw is as long as high, we could understand that the flaw is vertically oriented, and vertically oriented could be only a planar flaw.

 
 Reply 
 

Product Spotlight

HD-CR 35 NDT Computed Radiography System

Portable high-resolution CR scanner for all radiography applications - weld testing, profile images
...
and aerospace. No matter what type of radiographic testing you are performing, the unique TreFoc Technology of the HD-CR 35 NDT imaging plate scanner always guarantees the highest image quality.
>

SITEX CPSERIES

Teledyne ICM’s CPSERIES has been designed with a view to revolutionizing the handling and perfor
...
mances of portable X-Ray sets. Despite having managed to halve the weight of similar portable X-Ray generators available on the market (while continuing to provide the same power output), the SITEX CPSERIES generators feature a shutter, a laser pointer, a beryllium window, an aluminum filter and two integrated diaphragms (customized sizes are available upon request). Without compromising the robustness and reliability for which ICM products are renowned, the small size and light weight of the SITEX CPSERIES will radically change the way that you perform your RT inspections. And you will see a positive impact in terms of both quality and return on investment (ROI).
>

Compact NDT inspection-heads for measurements with active thermography

The compact inspection head is suitable for thermographic ndt tasks. The uncooled infrared camera
...
is specially developed for NDI-tasks and offers a thermal sensitivity until now known only from thermal imagers with cooled detector. All required components and functions are integrated into the inspection-head. You will only need an ethernet cable to connect the sensor with the evaluation system.
>

Research and Applications Development For NDT

The Research and Applications Development (RAD) group is a newly formed team within Acuren dedicat
...
ed to tackling challenging inspection problems. Our focus is the development of novel, field deployable, advanced inspection techniques for use in cases where standard NDT methods are ineffective. We don't wait for new innovations, we engineer them. From concept to commissioning.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window