C3 radiographic film acc. to EN 584-1

As many radiographers know the EN 584-1 standard distinguishes few radiographic film classes. Of coure film manufacturers have comply to the specification of the standard and thare can be several ways to obtain the C3 film class. In our laboratory we use Fuji IX 80 films and the manufacturer states that the film obtains C3 class if the development temperature is 26 deg C. If the temperature equals 28 deg C the film class is C4 ass to EN 584-1. There are some dificulties in getting the appropriate sensivity (it's hard to get the appropriate wire of the IQI - usually one is missing). We've tryied many solutions with other parameters of the examination i.e. voltage, time, screens, distance and many other...

The question apperas are we using the right film type? (of course it is C3 according to the producer). Maybe it would be advisable to change the film manufacturer to e.g. AGFA and this way the sensivity would increase? I don't state that the IQI wire is impossible to obtain on this film system (film and developer) but it usually is quite a hard task. Maybe You had the same problem and it has vanished after changing the film manufacturer?

We use IX80 Fuji films packed in a ruber cassette with 0,05mm front screen and 0,1mm rear lead screens

 
 Reply 
 
GOWRISANTHOSH PALIKA
NDT Inspector,
Royscan engineering pte ltd, Singapore, Joined May 2008, 52

GOWRISANTHOSH PALIKA

NDT Inspector,
Royscan engineering pte ltd,
Singapore,
Joined May 2008
52
03:36 Dec-16-2016
Re: C3 radiographic film acc. to EN 584-1
In Reply to sadek997 at 20:43 Apr-05-2011 (Opening).

hi
to get better sensitivity the recommended front lead screen 0.1mm to 0.2 mm in the range

 
 Reply 
 
Dr. Uwe Zscherpel
Director,
BAM Berlin, Germany, Joined Jan 2010, 83

Dr. Uwe Zscherpel

Director,
BAM Berlin,
Germany,
Joined Jan 2010
83
11:13 Dec-20-2016
Re: C3 radiographic film acc. to EN 584-1
In Reply to sadek997 at 20:43 Apr-05-2011 (Opening).

Dear Sadek,
we at BAM are doing NDT film system classifiction and certification for differerent film manufacturers. Fujifilm does not have BAM certificates. Our measurements showed since many years, that the Fujifilm IX 50 in standard NDT development conditiions (28 °C and 8 min cycle time) is in the C3 film system class and IX 80 is in the C4 system class. Of course, you can find development conditions (e.g. the weak Japanese Fujifilm Superdol developer at 25 °C and 11 min cycle time) which require longer X-ray exposure times to reach D=2. As a consequence, the IX80 film just imps in tyhe next class C3! But this are NOT the con ditions you find typically in Europe.
So, if you are searching for a C3 film system class I strongly recommend to use the Fujifilm IX50 type. Than you will also prevent any problems with the wire visibility, which should be very similar to AGFA D4 films.
If you are using X-rays for exposure, the lead screen thicknesses are sufficient, if you are using Ir-192 the suggested increased lead thicknesses should give better IQI visibilities.
Finally, are you aware that since 2012 EN 584 is no longer valid and replaced by ISO 11699?
Best regards
Uwe Z.

 
 Reply 
 

Product Spotlight

Magnetic X-Ray Pipeline Crawler

Zhong Yi brand pipeline crawler is magnetic/micro-video controlled crawler with DC X ray unit inst
...
alled for checking welding of pipeline. Move steadily inside the pipeline 6''-60''diameter with speed of up to 18m/min, Max. moving diatance 5 kilometers and provide the efficient inspection of the pipeline.
>

NovaScope 6000

The all-digital Novascope 6000 is a portable, ultra-high precision thickness gauge for high-speed
...
thickness measurement. Novascope 6000 has unmatched capabilities and unique features including: •Superior Resolution with high contrast, high-speed color RF display •High pulser voltage •Real-time video output •Increased internal/external data storage •Programmable SetUp features •Battery & AC Powered
>

Research Center IDEKO develops an ultrasonic train wheel inspection system for CAF

The Basque Research centre IK4-IDEKO has developed a state-of-the-art ultrasonic inspection system f
...
or the train wheel. This system secures a sound condition of train wheels and is thus a significant contribution to rail transport safety. The device was delivered to CAF recently and its use allows the manufacturer to become an approved supplier of rolling stock in Italy, as it meets the demanding homologation standards of this country. \\\\r\\\\n
>

High-end Ultrasonic Flaw Detector with 32:128PR PAUT and 2-ch TOFD: SyncScan 2

SIUI’s newly launched SyncScan 2, is a high-end ultrasonic flaw detector with 32:128PR PAUT and
...
2-ch TOFD, which can maximize your efficiency for PA and TOFD. ● Support PA/TOFD/UT ● 32-ch PA is more suitable for inspection on extra-thick wall and high-attenuation material. ● 32-ch PA and 2-ch TOFD work simultaneously. ● Support PR mode for corrosion inspection.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window