S S Ananthan
S S Ananthan
03:17 May-04-2002
Clad Thickness Measurement

Dear Sir,

I am in the lookout for an instrument for finding the thickness of cladding.
The base material is stainless steel AISI 309. The clad will be stellite 6 or stellite 21.
The thickness range will be about 1.0 to 2.0 mm. The accuracy levels required is 0.1 mm.
The clad is made with Gas Metal Arc Welding.

Can someone pl suggest a suitable equipment for this ?

S S Ananthan


 
 Reply 
 
Richard Kazares
Richard Kazares
05:39 May-04-2002
Re: Clad Thickness Measurement
It is SOMETIMES possible to detect a cladding layer using ultrasound - but it is usually not an easy task. The problem is the similarity of sound velocity (impedence) between the cladding and the base material.

Having noted the above - it MAY be possible to do so for specific conditions - if you wish, you can contact me (see e-mail) and we would be pleased to arrange to test a small sample of your material.


: Dear Sir,
.
: I am in the lookout for an instrument for finding the thickness of cladding.
: The base material is stainless steel AISI 309. The clad will be stellite 6 or stellite 21.
: The thickness range will be about 1.0 to 2.0 mm. The accuracy levels required is 0.1 mm.
: The clad is made with Gas Metal Arc Welding.
.
: Can someone pl suggest a suitable equipment for this ?
.
: S S Ananthan
.



 
 Reply 
 
S. White
S. White
03:34 May-06-2002
Re: Clad Thickness Measurement
You need to use eddy current.
It is widely used to measure coating thickness.
There are specific units that are sold that focus on measuring coating/cladding thickness.

: Dear Sir,
.
: I am in the lookout for an instrument for finding the thickness of cladding.
: The base material is stainless steel AISI 309. The clad will be stellite 6 or stellite 21.
: The thickness range will be about 1.0 to 2.0 mm. The accuracy levels required is 0.1 mm.
: The clad is made with Gas Metal Arc Welding.
.
: Can someone pl suggest a suitable equipment for this ?
.
: S S Ananthan
.



 
 Reply 
 
Tom Nelligan
Engineering,
retired, USA, Joined Nov 1998, 390

Tom Nelligan

Engineering,
retired,
USA,
Joined Nov 1998
390
09:31 May-06-2002
Re: Clad Thickness Measurement
As noted by Mr. Kazares, the success or failure of ultrasonic measurement of cladding thickness depends on the ratio of the acoustic impedances of the two materials. With stellite over stainless steel, there's a reasonably good chance that the mismatch will be sufficient to permit detection an echo with the proper equipment.

Simple ultrasonic gages will usually NOT make the measurement because they'll grab the very large echo off the bottom of the stainless rather than the much smaller echo from the stellite/stainless boundary.

I'd try a 20 MHz contact transducer (for fast recovery time) on either a flaw detector or a gage that allows the user to adjust gain and blanking. Note that because of the geometry of the boundary, the echo will be cleaner at some points than others, so I'd also recommend hunting around for the cleanest response before recording data.

--Tom Nelligan
Panametrics, Inc.


 
 Reply 
 
John Hart
John Hart
02:15 Aug-20-2002
low dilution clad technique - no melting substrate surface
: If you are interested in a low heat, low distortion and low dilution process which eliminates carrying a molten pool on the substrate surface for injection of cladding alloy, please contact H&R Technology. HRT's PMDTM process fuses solid metal flat wire onto a substrate without the need to create a molten pool of metal. As a result, HRT's PMDTM process repairs or produces metal parts with an order of magnitude less heat input than competing technologies, yielding parts with minimal distortion and superior metallurgical characteristics.

Dear Sir,
.
: I am in the lookout for an instrument for finding the thickness of cladding.
: The base material is stainless steel AISI 309. The clad will be stellite 6 or stellite 21.
: The thickness range will be about 1.0 to 2.0 mm. The accuracy levels required is 0.1 mm.
: The clad is made with Gas Metal Arc Welding.
.
: Can someone pl suggest a suitable equipment for this ?
.
: S S Ananthan
.



 
 Reply 
 
Sean Franklin
Sean Franklin
03:01 Aug-20-2002
Re: low dilution clad technique - no melting substrate surface
The NDT Automation M100A Metal Inspector uses resistivity to quickly and accurately record metal thickness (Metal to Metal & Metal to Non-Metal), metal sorting, as well as, several other applications such as spot/laser weld control.

The resistivity of metal is determined by its grain structure composition and state of internal stress.
The most common materials used in the metalworking industry have significantly different internal characteristics, and as a result, different resistivities.

For additional information contact Sean Franklin @ Sfranklin@NDTAutomation.com


: : If you are interested in a low heat, low distortion and low dilution process which eliminates carrying a molten pool on the substrate surface for injection of cladding alloy, please contact H&R Technology. HRT's PMDTM process fuses solid metal flat wire onto a substrate without the need to create a molten pool of metal. As a result, HRT's PMDTM process repairs or produces metal parts with an order of magnitude less heat input than competing technologies, yielding parts with minimal distortion and superior metallurgical characteristics.
.
: Dear Sir,
: .
: : I am in the lookout for an instrument for finding the thickness of cladding.
: : The base material is stainless steel AISI 309. The clad will be stellite 6 or stellite 21.
: : The thickness range will be about 1.0 to 2.0 mm. The accuracy levels required is 0.1 mm.
: : The clad is made with Gas Metal Arc Welding.
: .
: : Can someone pl suggest a suitable equipment for this ?
: .
: : S S Ananthan
: .
.



 
 Reply 
 

Product Spotlight

Wireless TOFD scanner

Quick, accurate and highly reproducible welds testing. The System operates wirelessly and is compat
...
ible with any type of Windows based Laptop, Desktop or Tablet.
>

32:128PR PAUT & 2-ch TOFD Flaw Detector: SyncScan 2

●32:128PR PAUT with optional 2-ch TOFD to maximize your efficiency ●Support PR mode for corrosi
...
on inspection ●Multiple solutions for welds & corrosion ●Faster scan speed (Approximately 3 meters/minute) ●Light weight: 4kg only including battery
>

Customized Probes and Transducers

With a strong development department and our own piezocomposite production, we accompany you from th
...
e first product idea to serial production. Our scientists are continuously researching new methods in the field of ultrasonic measurement technology. The progress achieved enables us to offer you optimal solutions.
>

PAUT Probes

Typical Phased Array probes have frequencies between 1MHz and 20MHz and the number of wafers is 10
...
to 128. M2 Electronics offers customers conventionally ultrasound probes and the ability to provide high-precision Phased Array Ultrasound Probes of up to 256 wafers. We can also customize the probe for our customers to meet the specific application requirements of the user.
>

Share...