03:34 Aug-12-2002
Thickness measurement

Hello everybody.
May somebody help me?
I need measure thickness of pipewall but I have one trouble.
Diameter of pipeline is 2500mm, and thickness of pipe wall is about 6-10mm.
I have apparatus DM-2LCDM with transducer DA211.
And what trouble?
This pipe is in blast furnance. Its leaning gas tubing.Entrance to the pipeline is only from one side(from above), and is impossible go round all pipe because its much high(60m).But I need measure all surface, but my hand is too short.(diameter 2500mm). Do you know how can I solve this trouble?
Thank you.
Milan
Sorry for my poor english.


 
 Reply 
 
Richard Kazares
Richard Kazares
06:44 Aug-12-2002
Re: Thickness measurement
You have an interesting problem - and I think we have a good solution for you - we manufacture a CONFIGURABLE magnetic scanner - that can easly go around the inside of a 2500 mm pipe - and perform a 100% thickness survery for you.

If you follow the link below to our website and get information on LSI (Large Structure Inspection) System.

It would be more than likely that we can help you perform this test - we have systems available for use in North America (4 systems), Europe (4 systems), the Middle East (1 system), South America (2 systems) and Japan (1 system).

Alternatively, you may contact me directly for more information.

Richard Kazares
General Manager
NDT Automation
1-619-716-4123

: Hello everybody.
: May somebody help me?
: I need measure thickness of pipewall but I have one trouble.
: Diameter of pipeline is 2500mm, and thickness of pipe wall is about 6-10mm.
: I have apparatus DM-2LCDM with transducer DA211.
: And what trouble?
: This pipe is in blast furnance. Its leaning gas tubing.Entrance to the pipeline is only from one side(from above), and is impossible go round all pipe because its much high(60m).But I need measure all surface, but my hand is too short.(diameter 2500mm). Do you know how can I solve this trouble?
: Thank you.
: Milan
: Sorry for my poor english.
.



 
 Reply 
 
S.V.Swamy
Engineering, - Material Testing Inspection & Quality Control
Retired from Nuclear Fuel Complex , India, Joined Feb 2001, 787

S.V.Swamy

Engineering, - Material Testing Inspection & Quality Control
Retired from Nuclear Fuel Complex ,
India,
Joined Feb 2001
787
07:30 Aug-13-2002
Re: Thickness measurement
From what Mr.Milan wrote, I got the impression that he cannot access the ID of the pipe, but can access the pipe only from OD and that too from above. In such a case, a magnetic crawler or a ring with the probe mounted by a spring so that contact is assured can be tried.

If he clarifies the access (from OD or ID), the solutions can be thought of.


: You have an interesting problem - and I think we have a good solution for you - we manufacture a CONFIGURABLE magnetic scanner - that can easly go around the inside of a 2500 mm pipe - and perform a 100% thickness survery for you.
.
: If you follow the link below to our website and get information on LSI (Large Structure Inspection) System.
.
: It would be more than likely that we can help you perform this test - we have systems available for use in North America (4 systems), Europe (4 systems), the Middle East (1 system), South America (2 systems) and Japan (1 system).
.
: Alternatively, you may contact me directly for more information.
.
: Richard Kazares
: General Manager
: NDT Automation
: 1-619-716-4123
.
.
: : Hello everybody.
: : May somebody help me?
: : I need measure thickness of pipewall but I have one trouble.
: : Diameter of pipeline is 2500mm, and thickness of pipe wall is about 6-10mm.
: : I have apparatus DM-2LCDM with transducer DA211.
: : And what trouble?
: : This pipe is in blast furnance. Its leaning gas tubing.Entrance to the pipeline is only from one side(from above), and is impossible go round all pipe because its much high(60m).But I need measure all surface, but my hand is too short.(diameter 2500mm). Do you know how can I solve this trouble?
: : Thank you.
: : Milan
: : Sorry for my poor english.
: .
.



 
 Reply 
 

Product Spotlight

Immersion systems

ScanMaster ultrasonic immersion systems are designed for high throughput, multi shift operation in a
...
n industrial or lab environment. These fully integrated systems provide various scanning configurations and incorporate conventional and phased arrays technologies to support diverse applications, such as inspection of disks, bars, shafts, billets and plates. All of ScanMaster immersion systems are built from high accuracy scanning frames allowing for scanning of complex parts and include a multi-channel ultrasonic instrument with exceptional performance. The systems are approved by all major manufacturers for C-scan inspection of jet engine forged discs. Together with a comprehensive set of software modules these flexible series of systems provide the customer with the best price performance solutions.
>

MUSE Mobile Ultrasonic Equipment

The MUSE, a portable ultrasonic imaging system, was developed for in-field inspections of light-weig
...
ht structures. The MUSE consists of a motor-driven manipulator, a water circulation system for the acoustic coupling and a portable ultrasonic flaw detector (USPC 3010). The MUSE provides images of internal defects (A-, B-,C- and D-scan).
>

Research Center IDEKO develops an ultrasonic train wheel inspection system for CAF

The Basque Research centre IK4-IDEKO has developed a state-of-the-art ultrasonic inspection system f
...
or the train wheel. This system secures a sound condition of train wheels and is thus a significant contribution to rail transport safety. The device was delivered to CAF recently and its use allows the manufacturer to become an approved supplier of rolling stock in Italy, as it meets the demanding homologation standards of this country. \\\\r\\\\n
>

HD-CR 35 NDT Computed Radiography System

Portable high-resolution CR scanner for all radiography applications - weld testing, profile images
...
and aerospace. No matter what type of radiographic testing you are performing, the unique TreFoc Technology of the HD-CR 35 NDT imaging plate scanner always guarantees the highest image quality.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window