Reflector plate testing

We employ reflector-plate testing on relatively thin (0.090" to 0.500") refractory metals. I would very much like to change to a back - surface reflection moniotoring type of test. Does anyone have any wisdom to contribute to this question? I understand some of the obvious differences, but I am somewhat stymied in coming up with the justification for trying to change over to this test. Thank you for your assistance.


 
 Reply 
 
Ed Ginzel
R & D, -
Materials Research Institute, Canada, Joined Nov 1998, 1300

Ed Ginzel

R & D, -
Materials Research Institute,
Canada,
Joined Nov 1998
1300
01:21 Mar-05-2003
Re: Reflector plate testing
Mr. Harvey:
Could you please provide a bit more information.
I am not clear on what "reflector-plate" testing is.
What are you monitoring or testing for. (Can I assume you are using some form of automated ultrasonic configuration?)
Ed

: We employ reflector-plate testing on relatively thin (0.090" to 0.500") refractory metals. I would very much like to change to a back - surface reflection moniotoring type of test. Does anyone have any wisdom to contribute to this question? I understand some of the obvious differences, but I am somewhat stymied in coming up with the justification for trying to change over to this test. Thank you for your assistance.
.




 
 Reply 
 
Carlos Valdecantos
Engineering
MTORRES, Ing., Spain, Joined May 2001, 9

Carlos Valdecantos

Engineering
MTORRES, Ing.,
Spain,
Joined May 2001
9
09:31 Mar-06-2003
Re: Reflector plate testing
As far as I understand, reflector plate test is also referred to as "double transmission" and gives no information about time of flight (thickness or flaw depth) because the echo being monitored is the one coming from the plate which is kept at a fixed distance from the transducer. Defects are shown in the C-scan as amplitude fall of the plate echo. Axial resolution is not involved, so standard transducer can be used. Although pulse-echo systems are used, reflector plate test is not strictly a pulse-echo test.

True pulse-echo test makes use the backwall echo of the part under test. This gives information on the amplitude (C-scan) and time of flight (D-scan), so thickness of the part and depth of defects are measured. High axial resolution transducers are required for thin parts testing. Also geometric requirements (perpendicularity to the part surface) are more stringent in pulse echo.


C. Valdecantos


 
 Reply 
 

Product Spotlight

MUSE Mobile Ultrasonic Equipment

The MUSE, a portable ultrasonic imaging system, was developed for in-field inspections of light-weig
...
ht structures. The MUSE consists of a motor-driven manipulator, a water circulation system for the acoustic coupling and a portable ultrasonic flaw detector (USPC 3010). The MUSE provides images of internal defects (A-, B-,C- and D-scan).
>

UCI Hardness Tester NOVOTEST T-U2

UCI hardness tester NOVOTEST T-U2 is is used for non-destructive hardness testing of: metals and
...
alloys by scales of hardness: Rockwell (HRC), Brinell (HB), Vickers (HV); non-ferrous metals, alloys of iron etc., and using five additional scales for calibration; with tensile strength (Rm) scale determines the tensile strength of carbon steel pearlitic products by automatic recalculation from Brinell (HB) hardness scale.
>

Ultrasonic Probe Recharacterization Service

NDT Systems offers a comprehensive Aftercare and Recharacterization Service for all our ultrasonic
...
probes. The Recharacterization Service is fully compliant with International ASTM E1065 Standard Guide (and other applicable standards) and offers complete documentation, traceable to the ASTM E1065 Standard. For more details or to schedule Recharacterization Services contact ndtsales@ndtsystems.com
>

SITEX CPSERIES

Teledyne ICM’s CPSERIES has been designed with a view to revolutionizing the handling and perfor
...
mances of portable X-Ray sets. Despite having managed to halve the weight of similar portable X-Ray generators available on the market (while continuing to provide the same power output), the SITEX CPSERIES generators feature a shutter, a laser pointer, a beryllium window, an aluminum filter and two integrated diaphragms (customized sizes are available upon request). Without compromising the robustness and reliability for which ICM products are renowned, the small size and light weight of the SITEX CPSERIES will radically change the way that you perform your RT inspections. And you will see a positive impact in terms of both quality and return on investment (ROI).
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window