02:06 May-05-2003
Measuring Stainless overlay 309L, 347L, 317L,316 etc.

Hello from South Carolina!!! well, once a year I go out to you all for you opinons on the above subject. Is there a system out there that can measure the thickness of Austentic overlay(ferrite)0.8 to 7.8 and it will vary. The welding application can vary also, but it is mostly automated. The backing is SA 285C or 516-70 mild steel (pressure vessels)or SA210 boiler tubes.For UT, the Z's factor is only 2. For magnetic induction or eddy current, the ferrite is the problem. We still measure befor overlay and after. The thickness will range from 1mm to 12mm.

Thankyou
M.C. Macke.


 
 Reply 
 
Doug Breeze
Director, Consultant; R&D
Inspection Software Limited, United Kingdom, Joined May 2000, 20

Doug Breeze

Director, Consultant; R&D
Inspection Software Limited,
United Kingdom,
Joined May 2000
20
08:44 Jun-05-2003
Re: Measuring Stainless overlay 309L, 347L, 317L,316 etc.
In response to Mike Macke's question a few weeks ago Dinsley Devices and Inspection Software have recently installed an automated system to measure Inconel cladding in the bore of 125mm - 300mm carbon steel pipe. Cladding thickness 0mm - 10mm, +/- 0.1mm. Should be suitable for other similar materials.



 
 Reply 
 

Product Spotlight

Portable Ground Penetrating Radar - Proceq GP8000

The Proceq GP8000 portable ground penetrating radar instrument is the beginning of a new era in ND
...
T. The outstanding, patented ultra- wideband technology combined with a compact wireless probe delivers unmatched industry performance. Proceq GP8000 is the world’s first large-scale inspection solution that utilizes Augmented Reality in industrial applications.
>

ISONIC 3510

Very Powerful Superior Performance Extremely Portable Smart Phased Array Ultrasonic Flaw Detector an
...
d Recorder with 2 Conventional UT and TOFD Channels uniquely combines PA, single- and multi-channel conventional UT, and TOFD modalities providing 100% raw data recording and imaging. Suitable for all kinds of every-day ultrasonic inspections
>

Ultrasonic Testing Immersion Tanks with Unmatched Scanning Features

TecScan’s non-destructive testing Ultrasonic Immersion Tanks & scanners are designed for high pe
...
rformance and demanding NDT testing applications. Our Scan3D™ line of High Precision Immersion Tanks are specifically designed for automated ultrasonic testing of complex composites parts used in aerospace and industrial applications.
>

IntraPhase Athena Phased Array System

The Athena Phased Array system, manufactured by WesDyne NDE Products & Technology, consists of a pha
...
sed array acquisition system and PC running IntraSpect software. A PC is used to perform acquisition, analysis and storage of the data. System hardware is capable of operating up to four data sets with any combination of phased array or conventional UT probes. NOW AVAILABLE IN 64-64 CONFIGURATION.
>