Technical Discussions
Diep eng Phan
NDT Inspector,
Vietnam, Joined Mar 2014, 10

Diep eng Phan

NDT Inspector,
Vietnam,
Joined Mar 2014
10
18:24 Aug-17-2014
Minimum thickness for Ultrasonic testing

Dear Sirs!

Please help me a problem follow as:
I don't know that minimum thickness for Ultrasonic testing in accordance with ASME BVP code how much?. Because some one said with me that, 6 mm is minimum thickness for ultrasonic testing in accordance with ASME BVP code. Please for me a advise, if this above is correct, please show me detail.
Thanks!

 
 Reply 
 
massimo carminati
Consultant, AUT specialist
IMG Ultrasuoni Srl, Italy, Joined Apr 2007, 691

massimo carminati

Consultant, AUT specialist
IMG Ultrasuoni Srl,
Italy,
Joined Apr 2007
691
08:36 Aug-18-2014
Re: Minimum thickness for Ultrasonic testing
In Reply to Diep eng Phan at 18:24 Aug-17-2014 (Opening).

I could not find any limitation on thickness on the ASME BPV code. Calling ASME BPV code is very general. Which section do you refer to? The only thickness related note I found on ASME VIII Div. 2 is Table 7.3 where you can see that for joints types 1,2,3 for shell thickness below 13 mm RT is the only option.
My personal judgment about minimum thickness is that with Manual UT the a.m. limitation is very wise. With AUT or SAUT methods using PA this can be safely and efficiently reduced down to the 6 mm you mentioned, or even slightly lower.

 
 Reply 
 
tinhaminhvt@yahoo.com
tinhaminhvt@yahoo.com
15:24 Aug-18-2014
Re: Minimum thickness for Ultrasonic testing
In Reply to Diep eng Phan at 18:24 Aug-17-2014 (Opening).

Dear Mr. Diep,

Just follow Special/ actual Specification you use. Cause by the death zone of your probe and material (mean death zone). So now, technical change rapidly, some new technique said that death zone is smaller (5 or 4mm).
You should follow Specification you refer, thay said 8mm, mean minimum 8mm, 6mm, mean 6mm.

 
 Reply 
 
PHAN HOANG DIEP
NDT Inspector,
Vietnam, Joined Mar 2014, 10

PHAN HOANG DIEP

NDT Inspector,
Vietnam,
Joined Mar 2014
10
17:56 Aug-18-2014
Re: Minimum thickness for Ultrasonic testing
In Reply to massimo carminati at 08:36 Aug-18-2014 .

Dear massimo carminati!
Thanks for your advise.
I have just seen at ASME VIII, 6 mm is minimum thickness for ultrasonic testing in lieu of radiography testing but no ASME VIII before 2007, that is ASME VIII 2013 Division I UW 51.
With my opinion, 6 mm is minimum thickness for UT in lieu of RT, actually depent on UT set manufacture combine with ASME committee to decision this problem.
please reply for me as soon as posible.
Mr Diep.

 
 Reply 
 
Bill
USA, Joined Jan 2010, 52

Bill

USA,
Joined Jan 2010
52
00:22 Aug-20-2014
Re: Minimum thickness for Ultrasonic testing
In Reply to PHAN HOANG DIEP at 17:56 Aug-18-2014 .

B31.3- No thickness limitation stated
CC-181- No thickness limmitation stated
B31.1- No thickness limitation stated
CC-189- No thickness limitation stated
Section 1-13mm min thickness
Section 8 Div 1 workmanship-no thickness limitation stated
Section 8 Div 1 use of Div 2 7.5.5- 6mm min thickness
Section 8 Div 2 workmanship- 13mm min thickness
Section 8 Div 2 7.5.5-13mm min thickness
CC 2235-13mm min thickness

All based on current code editions and not applicable to prior code editions.

Hope this helps

1
 
 Reply 
 
Pham Van Nam
Engineering,
oil&gas, Vietnam, Joined May 2014, 1

Pham Van Nam

Engineering,
oil&gas,
Vietnam,
Joined May 2014
1
08:27 Aug-20-2014
Re: Minimum thickness for Ultrasonic testing
In Reply to Bill at 00:22 Aug-20-2014 .

Dear all,

"Section 8 Div 1 use of Div 2 7.5.5- 6mm min thickness" but 7.5.5 use Section V - Mandatory VIII: Only apply for PAUT or TOFD, not for manual UT.

Finally, 13mm, do you agree?

 
 Reply 
 
Tuong
NDT Inspector, PV EIC NDT
PV EIC NDT, Vietnam, Joined Mar 2014, 19

Tuong

NDT Inspector, PV EIC NDT
PV EIC NDT,
Vietnam,
Joined Mar 2014
19
09:24 Aug-20-2014
Re: Minimum thickness for Ultrasonic testing
In Reply to massimo carminati at 08:36 Aug-18-2014 .

Right, 13mm. See cc 2235

 
 Reply 
 
Bill
USA, Joined Jan 2010, 52

Bill

USA,
Joined Jan 2010
52
20:24 Aug-20-2014
Re: Minimum thickness for Ultrasonic testing
In Reply to Pham Van Nam at 08:27 Aug-20-2014 .

No i do not agree. The minumum thickness for Section 8 Div 1 use of Div 2 7.5.5 is 6mm as I stated. Look at the text in Div 1 for yourself.

Section V Mandatory Appendix 8 is the requierments to follow when performing automated or semi-automated UT examination, for any technique, when a fracture mechanics based acceptance criteria is used. It is not limmited to PAUT or TOFD. For example automated or semi-automated conventional UT. Further it has nothing to do with UT thickness limitations in ASME. Any thickness limitation is set by the construction code itself.

Hope this helps

 
 Reply 
 
Bill
USA, Joined Jan 2010, 52

Bill

USA,
Joined Jan 2010
52
20:27 Aug-20-2014
Re: Minimum thickness for Ultrasonic testing
In Reply to Tuong at 09:24 Aug-20-2014 .

Dear Toung,

CC 2235 is its own document and the thickness limitation it states (13mm) is not applicable to all of ASME.

Hope this helps

 
 Reply 
 
Shank Vagal
India, Joined Jun 2014, 73

Shank Vagal

India,
Joined Jun 2014
73
01:30 Aug-21-2014
Re: Minimum thickness for Ultrasonic testing
In Reply to Bill at 20:27 Aug-20-2014 .

I would safely say, this limit depends on your system set up. You can not look in to any space < dead zone; size< near zone. So, why not follow these guidelines and conclude accordingly? I have done conventional UT on 4" dia x 5-6 mm A53 butts to ABS supervision in India- early 90s, I guess.

 
 Reply 
 

Product Spotlight

Lyft™: Pulsed Eddy Current Reinvented

PEC Reinvented—CUI Programs Redefined Corrosion under insulation (CUI) is possibly the greatest u
...
nresolved asset integrity problem in the industry. Current methods for measuring wall thickness with liftoff, without removing insulation, all have severe limitations. Eddyfi introduces Lyft — a reinvented, high-performance pulsed eddy current (PEC) solution. The patent- pending system features a state-of-the-art portable instrument, real- time C-scan imaging, fast data acquisition with grid-mapping and dynamic scanning modes, and flexibility with long cables. It can also scan through thick metal and insulation, as well as aluminum, stainless steel, and galvanized steel weather jackets. Who else but Eddyfi to reinvent an eddy current technique and redefine CUI programs. Got Lyft?
>

UCI Hardness Tester NOVOTEST T-U2

UCI hardness tester NOVOTEST T-U2 is is used for non-destructive hardness testing of: metals and
...
alloys by scales of hardness: Rockwell (HRC), Brinell (HB), Vickers (HV); non-ferrous metals, alloys of iron etc., and using five additional scales for calibration; with tensile strength (Rm) scale determines the tensile strength of carbon steel pearlitic products by automatic recalculation from Brinell (HB) hardness scale.
>

Ultrasonic tomograph for imaging of concrete structures А1040 MIRA

Applicable for concrete inspection allowing imaging of the internal structure of objects from conc
...
rete, reinforced concrete, different stones. The operation applies pulse-echo technique at one-side access to the object. The instrument is feasible for concrete inspection for searching conduct ducts, conduits, detection of foreign inclusions, holes, honeycombing, cracks and other concrete defects.
>

Navic - Steerable Modular Automated Scanner

The Navic is a modular, motorized, steerable scanner designed to carry multiple attachments used
...
in various scanning and inspection applications. The Navic is capable of weld scanning (girth welds and long seam welds), automated corrosion mapping, and tank scanning.
>