10:25 Oct-30-2014
Shear wave reference block for Rings

Need to fabricate a reference standard (Acceptance critereia is 2mm ) for inspecting alumiium ring of size 1200mm OD, 1100mm ID and 90 mm thick , pl suggest.

 
 Reply 
 
Dent
Consultant, NDE Manager NDELevel III/3
NDT Consultant, Canada, Joined Nov 1998, 250

Dent

Consultant, NDE Manager NDELevel III/3
NDT Consultant,
Canada,
Joined Nov 1998
250
12:02 Oct-30-2014
Re: Shear wave reference block for Rings
In Reply to Arivazhagan at 10:25 Oct-30-2014 (Opening).

It is normal to put notches ID & OD on the actual part for this type of inspection rather than make a special cal. block.

Your specification/procedure should be consulted.

 
 Reply 
 
Jawed Akhter
Jawed Akhter
16:23 Oct-30-2014
Re: Shear wave reference block for Rings
In Reply to Arivazhagan at 10:25 Oct-30-2014 (Opening).

Your stansard call for 2mm flat bottom hole of side drill hole ? in eithe case you need
reference block to set up sensitivity.

 
 Reply 
 
Dent
Consultant, NDE Manager NDELevel III/3
NDT Consultant, Canada, Joined Nov 1998, 250

Dent

Consultant, NDE Manager NDELevel III/3
NDT Consultant,
Canada,
Joined Nov 1998
250
21:24 Oct-30-2014
Re: Shear wave reference block for Rings
In Reply to Jawed Akhter at 16:23 Oct-30-2014 .

Subject line of posting is Shear Wave. FBH's are almost always for straight beam. SDH's are normally used for weld inspections.
Notches are used for angle beam examinations of various product forms including large forged rings like you describe. Unless you have additional material to make a cal block from it is common to put the notches in the actual product and if necessary machine them off after testing.

1
 
 Reply 
 
Simon Amallraja
Consultant, Advanced NDT Methods
Anu Consultants, India, Joined Aug 2013, 40

Simon Amallraja

Consultant, Advanced NDT Methods
Anu Consultants,
India,
Joined Aug 2013
40
10:00 Nov-03-2014
Re: Shear wave reference block for Rings
In Reply to Arivazhagan at 10:25 Oct-30-2014 (Opening).

You have couple of Ref Standard manufuacturers with NIST trecebaility.

Check with www.phtools.com. They will be able to support you immediately.

Good Luck

 
 Reply 
 

Product Spotlight

Robotic laser shearography enables 100% inspection of complex, flight-critical composite structures

An article in “Composites World Magazine” showcases Non Destructive Testing of aero-structures
...
with Laser Shearography. Over the years Dantec Dynamics has supplied many solutions for the aerospace industry. Referring to specific customer projects several of these cases are examined to outline the advantages of using Laser Shearography for automated defect detection.
>

Ultrasonic Squirter/Gantry System

TecScan’s NDT Ultrasonic Gantry Systems are industrial Squirter scanners designed for non-destru
...
ctive quality testing and raster scanning of large structures and parts. The Gantry Systems are usually composed of an Industrial Mechanical Scanner and a Control Room with System Workstation.
>

HARDNESS TESTER TKM-459CE combi

TKM-459CE combi applies 2 methods of hardness control: UCI and Leeb. It provides high-accuracy tes
...
ting of metals and alloys as well as items of different sizes and configurations, their hardened layers and galvanic coatings. Device represents results in HB, HRC, HV and others. Shock-, dust- and water-proof housing with intuitive software make this gauge easy to use in all working conditions.
>

EKOSCAN Phased Array

In order to always fit your needs, EKOSCAN can manufacture any type of UT transducer, either convent
...
ional or Phased Array. As an ISO 9001: 2015 certified company, EKOSCAN is extremely careful as far a material selection and manufacturing processes are concerned. Our probes guarantee our customers the benefits of latest innovations regarding piezo-composite, backing, impedance adaptation layer, etc. Specific probes for hostile environment: high temperature, high pressure, corrosive environment,etc. Specific probes designed to fit your specific application: optimization of every parameter to guarantee you the best detection.
>