Shear wave reference block for Rings

Need to fabricate a reference standard (Acceptance critereia is 2mm ) for inspecting alumiium ring of size 1200mm OD, 1100mm ID and 90 mm thick , pl suggest.

 
 Reply 
 
Dent
Consultant, NDE Manager NDELevel III/3
NDT Consultant, Canada, Joined Nov 1998, 250

Dent

Consultant, NDE Manager NDELevel III/3
NDT Consultant,
Canada,
Joined Nov 1998
250
12:02 Oct-30-2014
Re: Shear wave reference block for Rings
In Reply to Arivazhagan at 10:25 Oct-30-2014 (Opening).

It is normal to put notches ID & OD on the actual part for this type of inspection rather than make a special cal. block.

Your specification/procedure should be consulted.

 
 Reply 
 
Jawed Akhter
Jawed Akhter
16:23 Oct-30-2014
Re: Shear wave reference block for Rings
In Reply to Arivazhagan at 10:25 Oct-30-2014 (Opening).

Your stansard call for 2mm flat bottom hole of side drill hole ? in eithe case you need
reference block to set up sensitivity.

 
 Reply 
 
Dent
Consultant, NDE Manager NDELevel III/3
NDT Consultant, Canada, Joined Nov 1998, 250

Dent

Consultant, NDE Manager NDELevel III/3
NDT Consultant,
Canada,
Joined Nov 1998
250
21:24 Oct-30-2014
Re: Shear wave reference block for Rings
In Reply to Jawed Akhter at 16:23 Oct-30-2014 .

Subject line of posting is Shear Wave. FBH's are almost always for straight beam. SDH's are normally used for weld inspections.
Notches are used for angle beam examinations of various product forms including large forged rings like you describe. Unless you have additional material to make a cal block from it is common to put the notches in the actual product and if necessary machine them off after testing.

1
 
 Reply 
 
Simon Amallraja
Consultant, Advanced NDT Methods
Anu Consultants, India, Joined Aug 2013, 40

Simon Amallraja

Consultant, Advanced NDT Methods
Anu Consultants,
India,
Joined Aug 2013
40
10:00 Nov-03-2014
Re: Shear wave reference block for Rings
In Reply to Arivazhagan at 10:25 Oct-30-2014 (Opening).

You have couple of Ref Standard manufuacturers with NIST trecebaility.

Check with www.phtools.com. They will be able to support you immediately.

Good Luck

 
 Reply 
 

Product Spotlight

NEW! The PragmaPro Instrument Platform

The PragmaPro is based on a modular cartridge technology and supports various NDT instrument modal
...
ities such as UT, PAUT, ECT and many more. This new platform is based on a machined, powder-coated aluminum frame for shock-proofness, best sealing qualities and maximum heat dissipation. This is practical to extend the outdoor temperature range and/or to extend the power injected in the transducers. The PragmaPro is aiming at a very wide range of applications, such as weld scanning, corrosion mapping and composite testing.
>

Ultrasonic Testing Immersion Tanks with Unmatched Scanning Features

TecScan’s non-destructive testing Ultrasonic Immersion Tanks & scanners are designed for high pe
...
rformance and demanding NDT testing applications. Our Scan3D™ line of High Precision Immersion Tanks are specifically designed for automated ultrasonic testing of complex composites parts used in aerospace and industrial applications.
>

Aerospace Systems - Automated Ultrasonic Inspection

USL are specialists in the design and manufacture of turnkey ultrasonic inspection systems for aer
...
ospace applications. From monolithic composites to complex honeycomb structures. This video shows just a few examples of what is possible, find out more at: www.ultrasonic-sciences.co.uk
>

ISONIC 3510

Very Powerful Superior Performance Extremely Portable Smart Phased Array Ultrasonic Flaw Detector an
...
d Recorder with 2 Conventional UT and TOFD Channels uniquely combines PA, single- and multi-channel conventional UT, and TOFD modalities providing 100% raw data recording and imaging. Suitable for all kinds of every-day ultrasonic inspections
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window