Shear wave reference block for Rings

Need to fabricate a reference standard (Acceptance critereia is 2mm ) for inspecting alumiium ring of size 1200mm OD, 1100mm ID and 90 mm thick , pl suggest.

 
 Reply 
 
Dent
Consultant, NDE Manager NDELevel III/3
NDT Consultant, Canada, Joined Nov 1998, 252

Dent

Consultant, NDE Manager NDELevel III/3
NDT Consultant,
Canada,
Joined Nov 1998
252
12:02 Oct-30-2014
Re: Shear wave reference block for Rings
In Reply to Arivazhagan at 10:25 Oct-30-2014 (Opening).

It is normal to put notches ID & OD on the actual part for this type of inspection rather than make a special cal. block.

Your specification/procedure should be consulted.

 
 Reply 
 
Jawed Akhter
Jawed Akhter
16:23 Oct-30-2014
Re: Shear wave reference block for Rings
In Reply to Arivazhagan at 10:25 Oct-30-2014 (Opening).

Your stansard call for 2mm flat bottom hole of side drill hole ? in eithe case you need
reference block to set up sensitivity.

 
 Reply 
 
Dent
Consultant, NDE Manager NDELevel III/3
NDT Consultant, Canada, Joined Nov 1998, 252

Dent

Consultant, NDE Manager NDELevel III/3
NDT Consultant,
Canada,
Joined Nov 1998
252
21:24 Oct-30-2014
Re: Shear wave reference block for Rings
In Reply to Jawed Akhter at 16:23 Oct-30-2014 .

Subject line of posting is Shear Wave. FBH's are almost always for straight beam. SDH's are normally used for weld inspections.
Notches are used for angle beam examinations of various product forms including large forged rings like you describe. Unless you have additional material to make a cal block from it is common to put the notches in the actual product and if necessary machine them off after testing.

1
 
 Reply 
 
Simon Amallraja
Consultant, Advanced NDT Methods
Anu Consultants, India, Joined Aug 2013, 42

Simon Amallraja

Consultant, Advanced NDT Methods
Anu Consultants,
India,
Joined Aug 2013
42
10:00 Nov-03-2014
Re: Shear wave reference block for Rings
In Reply to Arivazhagan at 10:25 Oct-30-2014 (Opening).

You have couple of Ref Standard manufuacturers with NIST trecebaility.

Check with www.phtools.com. They will be able to support you immediately.

Good Luck

 
 Reply 
 

Product Spotlight

TESTD-PT SYSTEM

Pulse thermography is a non-contact test method that is ideal for the characterization of thin fil
...
ms and coatings or the detection of defects. With a remarquable short test time and a high detection sensitivity, the Telops TESTD-PT is the perfect tool for non- destructive testing. With such high frame rates, it is even possible to investigate highly conductive or diffusive materials.
>

IRIS 9000Plus - Introducing the next generation of heat exchanger inspection.

Representing the seventh generation of the IRIS system, the IRIS 9000 Plus has nearly 200 years of c
...
ombined field inspection experience incorporated in its design. This experience combined with a strong commitment to quality and a history of innovation has made Iris Inspection Services® the undisputed leader in IRIS technology.
>

OmniScan™ X3 flaw detector

The OmniScan X3 flaw detector is a complete phased array toolbox. Powerful tools, like total focus
...
ing method (TFM) images and advanced visualization capabilities, enable you to complete your inspection with greater confidence.
>

YXLON Cougar EVO

Scalable small footprint X-ray inspection systems for assembly and laboratory applications. The
...
YXLON Cougar EVO series was designed to provide the "best-in- class" inspection solutions for SMT, semiconductor, and laboratory assembly applications, while maintaining a small system footprint for maximum convenience. With optimized software and hardware, these systems produce higher quality and more consistent results than other electronics inspection systems currently on the market.
>

Share...
We use technical and analytics cookies to ensure that we will give you the best experience of our website - More Info
Accept
top
this is debug window